GB/T 19879 Q460GJC Building Steel Plate Supplier
What is GB/T 19879 Q460GJC Building Steel Plate?
Q460GJC, also written Q460GJ-C or Q460 GJC, is hot-rolled steel plate for building structures under GB/T 19879. Q means yield, 460 is the minimum yield in MPa, GJ (gao jian) marks high-performance building steel, and C is the quality grade: Charpy V-notch at 0°C, at least 47 J.
The GJ rules are what the structural engineer is paying for. Q460GJC sets a maximum yield as well as a minimum, caps the yield ratio, limits carbon equivalent by thickness and delivery route, and keeps P and S low. The frame then yields where the designer expects.
Q460GJC is the high-strength workhorse of Chinese super-tall towers. Published welding studies on the Ping An Finance Centre in Shenzhen describe all-position site welding of thick Q460GJC plate, which tells you where this grade lives: mega-columns and heavy nodes.
GB/T 19879-2023 replaced GB/T 19879-2015 on 1 April 2024. Q460GJ got its own CEV and Pcm limits in the 2015 edition. The 2023 edition keeps them, raises the yield-ratio cap from 0.83 to 0.85, uses ReH and holds 460–590 MPa to 100 mm. Chemistry, including Nb up to 0.110%, is unchanged. Sister grades are listed under GB/T 19879, including Q460GJB.
SHH STEEL (Shanghai Shenghonghe Import & Export Co., Ltd.) is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. We ship Q460GJC cut to size with an EN 10204 3.1 or 3.2 certificate.
Material Specification
| Specification element | Requirement | SHH STEEL compliance |
|---|---|---|
| Plate standard | GB/T 19879-2023 Q460GJC (GB/T 19879-2015 when the drawing names it) | Confirmed |
| Thickness for Q460GJ | 6 mm – 150 mm | Confirmed |
| Yield strength | 460 MPa min; 460 – 590 MPa for 16–100 mm | Confirmed |
| Tensile strength | 570 – 720 MPa (to 100 mm) | Confirmed |
| Yield ratio | ≤ 0.85 | Printed on MTC |
| Quality grade | C, Charpy V at 0°C, KV2 ≥ 47 J, longitudinal | Confirmed |
| Delivery condition | CR, NR, N, NT, QT, TMCP or TMCP+T | As ordered |
| Through-thickness | Z15, Z25 or Z35 to GB/T 5313 | As ordered |
| Dimensions | GB/T 709-2019, thickness tolerance Class B | Confirmed |
| Chemistry report | Heat analysis + CEV; product analysis on request | Confirmed |
| Certificate | EN 10204 3.1 or 3.2 | As ordered |
Grades often confused with it are GB/T 1591 Q460C and ASTM A572 Gr.65. None of them carries the GJ yield cap or yield-ratio rule.
Chemical Composition: Heat Analysis and Product Analysis
Two chemistry numbers exist for every Q460GJC plate. The mill reports the heat (ladle) analysis, which must sit inside Table 1. A check analysis drilled from the plate is the product analysis; clause 7.1.4 of GB/T 19879 lets it differ from Table 1 by the GB/T 222 deviations.
Table 1 below is the heat analysis for Q460GJC. The columns on the right show the quality-grade groups at Q460GJ.
Table 1. Heat (ladle) analysis, GB/T 19879-2023 Table 1, %
| Element | Q460GJC heat analysis (%) | Q460GJ B / C | Q460GJ D / E |
|---|---|---|---|
| C, max | 0.20 | 0.20 | 0.18 |
| Si, max | 0.55 | 0.55 | 0.55 |
| Mn, max | 1.70 | 1.70 | 1.70 |
| P, max | 0.025 | 0.025 | 0.020 |
| S, max | 0.015 | 0.015 | 0.010 |
| V, max | 0.200 | 0.200 | 0.200 |
| Nb, max | 0.110 | 0.110 | 0.110 |
| Ti, max | 0.030 | 0.030 | 0.030 |
| Als, min | 0.015 | 0.015 | 0.015 |
| Cr, max | 1.20 | 1.20 | 1.20 |
| Cu, max | 0.50 | 0.50 | 0.50 |
| Ni, max | 1.20 | 1.20 | 1.20 |
| Mo, max | 0.50 | 0.50 | 0.50 |
| V + Nb + Ti, max (if combined) | 0.22 | 0.22 | 0.22 |
Notes to Table 1. Total aluminium (Alt ≥ 0.020%) may replace acid-soluble aluminium. If Al, V, Nb or Ti is added alone or together at 0.015% or more, the minimum aluminium does not apply. V + Nb + Ti, when combined, is limited to 0.22%. These limits are the same in the 2015 and 2023 editions.
B and C grades share one chemistry column. D and E grades tighten carbon to 0.18%, phosphorus to 0.020% and sulfur to 0.010%, because they are tested at −20°C and −40°C.
Table 2. Product analysis limits for Q460GJC, GB/T 19879 clause 7.1.4 with GB/T 222-2025, %
| Element | Heat limit (%) | Permitted deviation, GB/T 222-2025 Table 1 | Q460GJC product analysis limit (%) |
|---|---|---|---|
| C | ≤ 0.20 | +0.02 | ≤ 0.22 |
| Si | ≤ 0.55 | +0.05 | ≤ 0.60 |
| Mn | ≤ 1.70 | +0.06 | ≤ 1.76 |
| P | ≤ 0.025 | +0.005 | ≤ 0.030 |
| S | ≤ 0.015 | +0.005 | ≤ 0.020 |
| V | ≤ 0.200 | +0.02 | ≤ 0.220 |
| Nb | ≤ 0.110 | ±0.005 | ≤ 0.115 (Table 1 lists Nb to 0.060%; agree above that) |
| Ti | ≤ 0.030 | +0.02 | ≤ 0.050 |
| Als | ≥ 0.015 | −0.003 | ≥ 0.012 |
| Cr | ≤ 1.20 | +0.05 | ≤ 1.25 |
| Cu | ≤ 0.50 | +0.05 | ≤ 0.55 |
| Ni | ≤ 1.20 | +0.05 | ≤ 1.25 (Table 1 covers Ni to 1.00%) |
| Mo | ≤ 0.50 | Not listed in Table 1 | Agree in contract (alloy-steel Table 2 would give ≤ 0.52) |
How to read Table 2. The band is chosen by the Table 1 upper limit. Si ≤0.55% is above 0.37%, so +0.05% applies; Mn ≤1.70% falls in the 0.80–1.70% band, so +0.06%. For one heat an element may deviate in one direction only. Ni up to 1.20% is beyond the 1.00% range of Table 1; we apply the alloy-steel figure (±0.05%), which gives the same limit.
GB/T 222-2025 replaced GB/T 222-2006 on 1 December 2025. One more rule from it matters to buyers: if no reliable heat analysis exists, the product analysis must meet the heat limits with no deviation at all (clause 5.6).
Z-grade plate is cleaner still. GB/T 5313-2023 limits sulfur by heat analysis:
| Z grade | Heat sulfur, max (%) | Reduction of area, avg / single (%) |
|---|---|---|
| Z15 | 0.010 | 15 / 10 |
| Z25 | 0.007 | 25 / 15 |
| Z35 | 0.005 | 35 / 25 |
CEV and Pcm are always worked out from the heat analysis, not the product analysis. SHH STEEL prints the heat values used and adds a product-analysis column on request. This is building steel, not boiler chemistry such as GB/T 713 Q345R in GB/T 713.
Mechanical Properties
Values below follow Table 3 and Table 5 of GB/T 19879-2023 for Q460GJ. Tensile specimens are transverse; Charpy specimens are longitudinal.
| Thickness | Upper yield ReH (MPa) | Tensile Rm (MPa) | Yield ratio, max | Elongation A, min |
|---|---|---|---|---|
| 6 – 16 mm | ≥ 460 | 570 – 720 | 0.85 | 18% |
| > 16 – 100 mm | 460 – 590 | 570 – 720 | 0.85 | 18% |
| > 100 – 150 mm | 440 – 570 | 550 – 700 | 0.85 | 18% |
The 2015 edition used lower yield ReL and stepped yield down 10 MPa above 50 mm. Write the edition on the order so the mill tests to the right table.
| Test | Q460GJC requirement |
|---|---|
| Charpy V-notch, longitudinal | 0°C, KV2 ≥ 47 J, average of 3 |
| Single value | One value may fall below the average requirement, not below 70% of it (GB/T 17505) |
| Sub-size specimens | 7.5 mm or 5 mm wide when plate is too thin: 75% or 50% of the required energy |
| 180° bend | Per Table 6 to GB/T 232; may be omitted when the mill guarantees it (7.4.3.2) |
| Through-thickness (≥ 15 mm) | Z15, Z25 or Z35 to GB/T 5313, when ordered |
Density for theoretical weight is 7.85 g/cm³.
Q460GJC vs S460 (N, M and Q): Which 460 MPa Plate Fits a Building Frame?
European engineers reviewing a Chinese tower often ask whether Q460GJC is just S460. It is not. S460N and S460M give 460 MPa on thin plate and step down with thickness; S460Q holds yield longer but has no ceiling. None of them limits the yield ratio.
Q460GJC keeps 460–590 MPa from 16 mm to 100 mm and caps the ratio at 0.85. That is a seismic-design requirement, not a strength upgrade.
| Property | S460N / S460M | S460Q (EN 10025-6) | Q460GJC (GB/T 19879-2023) |
|---|---|---|---|
| Delivery | Normalized / TMCP | Quenched + tempered | CR, NR, N, NT, QT or TMCP |
| Yield at 16 mm | 460 MPa | 460 MPa | 460 MPa |
| Yield at 40–63 mm | 430 MPa min | 460 MPa min (to 50 mm) | 460 – 590 MPa |
| Yield at 80–100 mm | 400 MPa min | 440 MPa min | 460 – 590 MPa |
| Yield upper limit | None | None | 590 MPa to 100 mm |
| Yield ratio | No limit | No limit | ≤ 0.85 |
| Impact | N/M −20°C 40 J; NL/ML −50°C 27 J | Q −20°C; QL −40°C; QL1 −60°C | 0°C, 47 J |
For 0°C service, EN 10025-3 S460N and GB/T 1591 Q460C are the usual strength comparisons. Our QT reference grade is GB/T 16270 Q460C.
Closest single comparison for Q460GJC: EN 10025-3 S460N, strength only.
N, TMCP or QT? Choosing the Delivery Route for Q460GJC
| Route (GB/T 19879-2023) | CEV ≤ 50 / 50–100 / 100–150 mm | Pcm ≤ 50 / 50–100 / 100–150 mm | What it means in the shop |
|---|---|---|---|
| CR, NR, N, NT | 0.52 / 0.54 / 0.56% | 0.32 / 0.34 / 0.35% | Highest CEV; more preheat on thick plate |
| QT | 0.45 / 0.48 / 0.50% | 0.28 / 0.30 / 0.31% | Lower CEV, full-thickness strength; heat-input limits matter |
| TMCP, TMCP+T | 0.42 / 0.45 / by agreement | 0.27 / by agreement | Lowest CEV; best weldability to 100 mm |
The same grade name covers three very different plates. A 100 mm normalized Q460GJC plate can carry CEV 0.54%; a TMCP plate of the same thickness, 0.45%. The fabricator’s preheat, interpass and consumable choice follow that number.
We put the route on the quotation. If the drawing is silent, we recommend TMCP up to about 80 mm and QT for the heaviest plate, then let the welding engineer confirm.
Q460GJB, Q460GJC, Q460GJD or Q460GJE: Which Quality Grade?
| Grade | Impact temperature | Energy, min | C / P / S max (%) | Typical use |
|---|---|---|---|---|
| Q460GJB | +20°C | 47 J | 0.20 / 0.025 / 0.015 | Heated interiors, mild climates |
| Q460GJC | 0°C | 47 J | 0.20 / 0.025 / 0.015 | Cold regions, exposed frames |
| Q460GJD | −20°C | 47 J | 0.18 / 0.020 / 0.010 | Severe winters, thick welded nodes |
| Q460GJE | −40°C | 47 J | 0.18 / 0.020 / 0.010 | Arctic and low-temperature sites |
Strength, yield ratio and CEV do not change from B to E. Only the impact temperature and the D/E chemistry move. The letter should follow the coldest temperature the steel will see, during erection as well as in service.
Q460GJC is the usual letter for temperate sites and for frames that see some frost during erection. For the same letter at another strength level: one level up, Q500GJC; one level down, Q420GJC.
Q460GJCZ15, Q460GJCZ25 and Q460GJCZ35: Through-Thickness Plate
Lamellar tearing starts inside the plate, parallel to the surface, when a large weld pulls on it through the thickness. Box-column diaphragms and T-joints on thick flanges are the classic cases. A Z grade is the guarantee against it.
The designation adds the Z level to the grade, for example Q460GJCZ25. Z tests apply to plate 15 mm and thicker and follow GB/T 5313-2023.
| Z grade | Heat sulfur, max (%) | Reduction of area, avg / single (%) |
|---|---|---|
| Z15 | 0.010 | 15 / 10 |
| Z25 | 0.007 | 25 / 15 |
| Z35 | 0.005 | 35 / 25 |
B and C chemistry allows S up to 0.015%, so even Z15 needs extra desulfurization.
GB/T 19879-2023 clause 7.6 requires every Z plate to be ultrasonic tested one by one to GB/T 2970, acceptance level III. Z35 costs most: lowest sulfur, more rejects, and a Z test on each plate.
Our advice: mark Z25 or Z35 on the cutting list by member, not on the whole order. Stiffeners and webs rarely need it.
Equivalent Material Grades
ASTM A913 Gr.65 is the US high-strength seismic shape grade; it is a section standard, not plate. For plate, A572 Gr.65 is the strength comparison.
| Designation | Region | Standard | Notes |
|---|---|---|---|
| Q460GJC | China | GB/T 19879-2023 | Grade on this page |
| EN 10025-3 S460N | Europe | EN 10025-3/-4 | Strength match; no yield cap |
| EN 10025-4 S460M | Europe | EN 10025-3/-4 | Alternative route |
| EN 10025-6 S460Q | Europe | EN 10025-6 | QT; holds yield to 50 mm |
| GB/T 1591 Q460C | China | GB/T 1591-2018 | General structural |
| GB/T 16270 Q460C | China | GB/T 16270 | QT plate |
| ASTM A572 Gr.65 | USA | ASTM A572 | 450 MPa; one step lower |
| JIS G3106 SM570 | Japan | JIS G3106 | About 450–460 MPa; −5°C impact |
On EN projects we usually quote Q460GJC against S460M or S460ML, because the TMCP route also gives the lowest CEV. See EN 10025-4 and EN 10025-6.
Weldability
GB/T 19879 makes the mill calculate CEV from the heat analysis and print it, together with the elements used, on every Q460GJC certificate:
CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15
Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B
| Delivery condition | CEV ≤ 50 mm | CEV > 50 – 100 mm | CEV > 100 – 150 mm | Pcm ≤ 50 mm | Pcm > 50 – 100 mm | Pcm > 100 – 150 mm |
|---|---|---|---|---|---|---|
| CR, NR, N, NT | 0.52 | 0.54 | 0.56 | 0.32 | 0.34 | 0.35 |
| QT | 0.45 | 0.48 | 0.50 | 0.28 | 0.30 | 0.31 |
| TMCP, TMCP+T | 0.42 | 0.45 | By agreement | 0.27 | By agreement | — |
Q460GJ needs a written procedure. Published work on thick Q460GJC site welding reports preheat around 120°C, with interpass control and low-hydrogen consumables. Use that as context, not as your WPS.
B/C chemistry allows C up to 0.20%. Check actual CEV on the MTC, not the table limit, when setting preheat.
Typical consumables: E55- or E62-class low-hydrogen electrodes (GB/T 5118) or matching gas-shielded and SAW wires. Shops work to GB 50661 or AWS D1.1. Write the CEV basis (actual heat, not table maximum) into the WPS.
Heat Treatment and Delivery Condition
Q460GJC may be delivered CR, NR, N or NT, QT, or TMCP / TMCP+T. QT is also permitted. Each route has its own CEV and Pcm limits, so the route is part of the specification, not a mill detail.
TMCP gives the lowest CEV and the best weldability. N or NT gives the most uniform through-thickness properties on heavy plate. QT holds strength in the thickest sizes.
Agree the route before price. A mill quoting N where the drawing assumed TMCP CEV is not quoting the same plate. TMCP references: GB/T 1591 Q460MC; normalized: GB/T 1591 Q460NC.
Test lots follow clause 9.2 of GB/T 19879-2023; retests and judgement follow GB/T 17505.
Dimensions
Q460GJC sizes we supply from mill and stock:
- Thickness: 6 mm – 150 mm; most orders 8 mm – 100 mm
- Width: 1500 mm – 3000 mm standard; wider by mill confirmation
- Length: 3000 mm – 12000 mm; longer by enquiry
- Edge: mill edge or cut edge
- Weight: theoretical, on the mean of maximum and minimum thickness, 7.85 g/cm³
Column flanges, diaphragms, stiffeners and gussets are cut to drawing. Rolled sections for the same frame are under steel beam profiles and steel structural profiles.
Tolerances
Dimensional tolerances for Q460GJC come from GB/T 709-2019, as GB/T 19879 directs. The default is Class B, which fixes the minus side at 0.30 mm. Ask for Class C if the design cannot accept any minus.
| Nominal thickness (mm) | Width ≤ 1500 mm | Width > 1500 – 2500 mm |
|---|---|---|
| > 8 – 15 | −0.30 / +0.80 | −0.30 / +1.00 |
| > 15 – 25 | −0.30 / +1.00 | −0.30 / +1.20 |
| > 25 – 40 | −0.30 / +1.10 | −0.30 / +1.30 |
| > 40 – 60 | −0.30 / +1.30 | −0.30 / +1.50 |
| > 60 – 100 | −0.30 / +1.50 | −0.30 / +1.80 |
| > 100 – 150 | −0.30 / +2.10 | −0.30 / +2.50 |
Flatness and width follow GB/T 709. EN 10029 or ASTM A6 tolerances are possible if written on the order.
Supplementary Requirements
Q460GJC already fixes strength, yield ratio, CEV and 0°C impact. Anything more goes on the purchase order.
- Edition: GB/T 19879-2023 or -2015. Never write only Q460.
- Product analysis: ask for a second chemistry column checked to GB/T 222.
- Through-thickness: add Z15, Z25 or Z35, e.g. Q460GJCZ25.
- Delivery condition: name it (CR, NR, N, NT, QT, TMCP or TMCP+T) if the welding procedure depends on it.
- Ultrasonic testing beyond Z plates: GB/T 2970 class, or EN 10160 / ASTM A578.
- Impact: extra test positions (e.g. quarter thickness) or transverse tests, if the owner wants them beyond the C letter.
- Tolerance: Class C for zero minus.
- Inspection: EN 10204 3.2 with SGS, BV, TÜV or a named inspector.
Q460GJC Price Factors and How to Order
Two Q460GJC quotes can differ by a lot and both be fair. The base price is similar across mills; the extras below are where they part.
| Cost driver | Effect on price |
|---|---|
| GJ grade over general Q460 plate | Grade extra for cleaner steel, yield control and CEV |
| Quality letter C | Small extra for 0°C testing |
| Delivery route | QT and TMCP carry the largest route extras |
| Thickness | Thin and very thick plate carry size extras; 10–60 mm is usually cheapest |
| Z15 / Z25 / Z35 | Desulfurization, plate-by-plate Z test and UT; Z35 costs most |
| Width and length | Over 3000 mm wide or 12 m long needs mill confirmation |
| Quantity per size | Mill rolling minimums per size; small lots come from stock or combined rolling |
| Inspection and cutting | 3.2 witness, profile cutting, blasting and priming are quoted per item |
To get a firm quote in one round, send:
- Grade and edition, e.g. Q460GJCZ25 to GB/T 19879-2023
- Thickness × width × length and pieces or tonnes
- Delivery route, UT standard and class
- Certificate type and inspector
- Destination port and Incoterm
We quote plate price, extras and freight line by line, so you can compare like with like. Need a different letter? See Q460GJE.
Applications
| Sector | Typical Q460GJC components |
|---|---|
| Super-tall towers | Mega-columns, outrigger nodes, heavy splices |
| Stadium and terminal roofs | Main truss chords and support nodes |
| Transfer structures | Heavily loaded transfer and hanger plates |
| Steel-concrete composite | Plate for encased or concrete-filled mega-columns |
C grade suits frames that see winter during erection or in service, and exposed members in temperate climates.
It is the wrong plate for pressure equipment (pressure vessel steel plates), for bare exposed steel (weathering steel plates) or for ship hulls (shipbuilding steel plates).
Supply Capability and Global Delivery
SHH STEEL sources Q460GJC from first-line building-steel mills: Wuyang (Wugang), a drafting mill of GB/T 19879, plus Xinyu, Valin Xiangtan, Shougang, Puyang and Hongchang when size requires.
- Certificates: EN 10204 3.1 standard; 3.2 with third-party witness
- Tests: tensile, 0°C Charpy, bend, Z test to GB/T 5313, UT to GB/T 2970, product analysis
- Processing: CNC plasma and flame cutting, bevelling, drilling, shot blast and primer
- Terms: FOB Shanghai, CFR, CIF; TT, LC or TT + LC
- Marking: steel-stamped and paint-marked with grade, heat, size and mill
Q460GJC leaves Shanghai for projects designed to Chinese codes abroad, mostly through EPC contractors in Southeast Asia, the Middle East and Africa. We also ship ASTM, ASME, EN, DIN and JIS plate to Europe and the Americas.
Lead time: stock sizes about 5–7 days (B/C letters); mill rolling about 30–45 days; Z35 or 3.2 inspection adds about 1–2 weeks. Sea time from Shanghai is about 7–12 days to Singapore and 28–35 days to Rotterdam.
Why Choose SHH STEEL
SHH STEEL works mill-direct as a steel manufacturer and exporter and global steel mill sourcing partner, China origin. With Q460GJC you get the GJ plate the drawing asks for, traced to the heat.
Before shipment we check four lines on every certificate: yield inside the GJ window, yield ratio within the cap, CEV inside the thickness band for the delivery route, and 0°C impact at 47 J or more. If one fails, the plate does not ship as GJ.
We also tell buyers when they are over-specifying. If the design can live with 420 MPa, Q420GJC saves preheat and price. Browse more structural steel plates and high strength low alloy plates.
FAQ
-
What is Q460GJC steel?
- Q460GJC is high-performance building structure steel plate to GB/T 19879. It has 460 MPa minimum yield, a 460–590 MPa yield window from 16 to 100 mm, yield ratio ≤0.85, CEV limits by delivery route and Charpy impact of at least 47 J at 0°C. GJ stands for gao jian, high-performance building steel.
-
What is the difference between Q460GJC and S460N?
- S460N (EN 10025) has a 460 MPa minimum yield that falls with thickness and no yield cap or yield-ratio limit. Q460GJC (GB/T 19879-2023) holds 460–590 MPa from 16 to 100 mm, caps the yield ratio at 0.85, sets CEV by delivery route and needs 47 J at 0°C. They are comparable for strength, not interchangeable.
-
What impact test does Q460GJC require?
- Q460GJC needs Charpy V-notch tests at 0°C on longitudinal specimens, with an average of at least 47 J from three tests. Plate too thin for a full 10 mm specimen is tested at 7.5 mm or 5 mm width, needing 75% or 50% of 47 J. The test applies to plate 6 mm and thicker.
-
Is Q460GJ the same as Q460 in GB/T 1591?
- No. GB/T 1591 Q460 has a minimum yield that falls with thickness and no yield cap or ratio limit; hot-rolled Q460 also starts at grade C. Q460GJ (GB/T 19879) holds 460–590 MPa from 16 to 100 mm, caps the ratio at 0.85 and needs 47 J.
-
What is the CEV limit of Q460GJC?
- Under GB/T 19879-2023 Table 2, Q460GJC up to 50 mm is capped at CEV 0.52% (CR, NR, N, NT); TMCP plate at 0.42%. CEV = C + Mn/6 + (Cr+Mo+V)/5 + (Ni+Cu)/15, from the heat analysis.
-
What is the ASTM or EN equivalent of Q460GJC?
- For strength, Q460GJC is compared with EN 10025 S460N/M or S460Q, ASTM A572 Gr.65 (450 MPa) and JIS SM570. None is an exact equivalent: they have no 590 MPa yield cap or 0.85 yield-ratio limit, which GB/T 19879-2023 requires for Q460GJC.
Conclusion
Q460GJC steel plate to GB/T 19879 is building structure plate with 460 MPa minimum yield, a capped yield window, a yield-ratio limit and 47 J impact at 0°C. It shares its chemistry with Q460GJB but proves toughness at its own letter. It is not general structural plate under GB/T 1591.
Every Q460GJC plate from SHH STEEL ships with heat analysis, CEV, yield and yield ratio, and Charpy results on an EN 10204 3.1 or 3.2 certificate. Product analysis to GB/T 222, Z15–Z35, UT to GB/T 2970, Class C tolerance and cut-to-size are options.
We ship from Shanghai to buyers worldwide. Browse the full GB/T 19879 range or other carbon steel plates.
Share your size list, Z level, quality letter and the edition on the drawing, and we reply with the mill, delivery route, lead time, test plan and price in one message. Contact SHH STEEL for a mill-direct Q460GJC building steel plate quotation.