Q420C Steel Plate GB/T 1591 Supplier
What is Q420C steel plate GB/T 1591?
Q420C is a 420 MPa hot-rolled HSLA plate impact-tested at 0°C. In GB/T 1591-2018 the hot-rolled Q420 family only has two quality letters, B and C, so Q420C is the tougher of the two. For −20°C or −40°C service the standard sends you to the N or M delivery conditions such as Q420NC or Q420MC.
Q420C is popular for high-rise building columns, transmission towers, heavy truck chassis and mining structures where engineers want more strength than Q390NC class plates without moving to quenched and tempered steel.
SHH STEEL is a producer and exporter of structural plate and a sales agent for well-known Chinese mills. We keep Q420C plate in our own processing warehouse in Shanghai for cutting, drilling, shot blasting and priming. Q420C belongs to our GB/T 1591 plate range; see also our high-strength low-alloy plates overview.
Q420C specification at a glance
| Item | Q420C requirement |
|---|---|
| Standard | GB/T 1591-2018, hot-rolled (AR) condition |
| Steel type | High-strength low-alloy structural steel, killed |
| Minimum yield ReH (≤16 mm) | 420 MPa |
| Tensile strength Rm (≤100 mm) | 520 – 680 MPa |
| Impact test | KV2 ≥ 34 J at 0°C, longitudinal |
| Thickness range (SHH STEEL) | 6 – 150 mm |
| Width / length | 1 500 – 4 020 mm / 6 000 – 18 000 mm |
| Dimensions & tolerance | GB/T 709 (EN 10029 / ASTM A6 on request) |
| Certificate | EN 10204 3.1 (3.2 with third-party inspection) |
Q420C chemical composition (heat analysis)
| Element | Q420C heat analysis, % max | Role |
|---|---|---|
| C | ≤ 0.20 | strength and hardenability; kept ≤0.20 for weldability |
| Si | ≤ 0.55 | deoxidiser, adds some strength |
| Mn | ≤ 1.70 | main strengthening element; with C sets the CEV |
| P | ≤ 0.030 | impurity; lower in the tougher quality letters |
| S | ≤ 0.030 | impurity; forms MnS that hurts through-thickness and impact values |
| Nb | ≤ 0.05 | grain refiner, precipitation strengthening |
| V | ≤ 0.13 | precipitation strengthening, helps thick plate keep yield |
| Ti | ≤ 0.05 | fixes N, refines grain in the HAZ |
| Cr | ≤ 0.30 | residual / minor alloy |
| Ni | ≤ 0.80 | residual; helps low-temperature toughness |
| Cu | ≤ 0.40 | residual; limited for hot shortness |
| Mo | ≤ 0.20 | residual / minor alloy |
| N | ≤ 0.015 | kept low; free N harms toughness |
Grade C tightens P and S to 0.030% each. Nb, V and Ti may be used alone or in combination; for Q390/Q420 the sum Nb+V+Ti is limited to 0.22%. Where Cu is used as a residual element the mill must report it. Values are for the ladle (heat) analysis printed on the certificate.
Product (finished plate) analysis and check tolerances for Q420C
A check analysis drilled from the finished plate may differ slightly from the ladle analysis. GB/T 1591 refers to GB/T 222 for the permitted deviations. The table applies them to the Q420C limits. The deviation applies to one side of a limit only.
| Element | Heat analysis limit, % | Permitted deviation | Product analysis limit, % |
|---|---|---|---|
| C | ≤ 0.20 | +0.02 | ≤ 0.22 |
| Si | ≤ 0.55 | +0.03 | ≤ 0.58 |
| Mn | ≤ 1.70 | +0.1 | ≤ 1.80 |
| P | ≤ 0.030 | +0.005 | ≤ 0.035 |
| S | ≤ 0.030 | +0.005 | ≤ 0.035 |
| Nb | ≤ 0.05 | +0.01 | ≤ 0.06 |
| V | ≤ 0.13 | +0.02 | ≤ 0.15 |
| Ti | ≤ 0.05 | +0.01 | ≤ 0.06 |
| Cr | ≤ 0.30 | +0.05 | ≤ 0.35 |
| Ni | ≤ 0.80 | +0.05 | ≤ 0.85 |
| Cu | ≤ 0.40 | +0.05 | ≤ 0.45 |
| Mo | ≤ 0.20 | +0.01 | ≤ 0.21 |
| N | ≤ 0.015 | +0.002 | ≤ 0.017 |
If your inspector tests a plate in a third-party lab, compare the result with the right-hand column, not with the heat analysis.
Q420C mechanical properties by thickness
| Thickness, mm | Yield ReH, MPa min | Tensile Rm, MPa | Elongation A, % min (long. / trans.) |
|---|---|---|---|
| ≤ 16 | 420 | 520 – 680 | 20 / – |
| > 16 – 40 | 410 | 520 – 680 | 20 / – |
| > 40 – 63 | 390 | 520 – 680 | 19 / – |
| > 63 – 100 | 370 | 520 – 680 | 19 / – |
| > 100 – 150 | 350 | 500 – 650 | 19 / – |
| Quality | Test temperature | KV2 longitudinal, J min | KV2 transverse, J min |
|---|---|---|---|
| C | 0°C | 34 | 27 |
Yield drops with thickness because thick plate cools slower and gets less rolling reduction. Design with the value for your actual thickness, not the headline 420 MPa. Impact tests use 10×10 mm specimens for plate ≥ 12 mm; thinner plate uses sub-size specimens with reduced values. Tensile tests on plate are transverse by default.
Q420C carbon equivalent (CEV) and weldability
| Thickness, mm | ≤ 30 | > 30 – 63 | > 63 – 150 | > 150 – 250 |
|---|---|---|---|---|
| CEV max, % (heat analysis) | 0.45 | 0.47 | 0.48 | 0.49 |
CEV = C + Mn/6 + (Cr+Mo+V)/5 + (Ni+Cu)/15. Real heats from our mills usually come in around 0.42 – 0.46 on 20 – 40 mm plate. Q420 plate welds with standard E50/E55-class consumables (AWS E7018 / E8018 type, ER50-6 / ER55 wire). Preheat of 50 – 100°C is common above 25 mm or in restrained joints; low-hydrogen practice is the key point.
Q420C equivalent grades: EN, ASTM, JIS
| System | Grade | Comment |
|---|---|---|
| EN 10025-3 | EN 10025-3 S420N | Normalized 420 MPa, −20°C 40 J; tougher than Q420C |
| ASTM | ASTM A572 Gr.60 | 415 MPa yield; impact only by S5 |
| GB/T 1591-2018 | Q420NC / Q420MC | N and M versions |
| EN 10025-2 | EN 10025-2 S355J0 | Lower strength, 0°C – not a swap |
“Equivalent” means similar, not identical. Strength classes, impact temperatures and delivery conditions differ between standards. A plate can be dual-certified only if one heat meets both books in full; ask us before you assume it.
Q420C vs Q420B vs Q460C
| Grade | Yield ≤16 mm, MPa | Tensile ≤100 mm, MPa | Impact |
|---|---|---|---|
| Q420B | 420 | 520 – 680 | +20°C |
| Q420C | 420 | 520 – 680 | 0°C |
| Q460C | 460 | 550 – 720 | 0°C |
Q420C vs Q420B: same strength, test at 0°C instead of +20°C, P and S 0.030%. Q420C vs Q460C: Q460C adds 40 MPa and is the last hot-rolled grade in GB/T 1591-2018. Q420C vs Q420D: for −20°C service.
Q420C applications in construction and machinery
Q420C plate is used for high-rise building columns and transfer trusses, power transmission towers, heavy truck chassis and trailer beams, mining and port equipment, stadium roof structures.
For building columns with through-thickness loads, compare with Q390GJC building plate to GB/T 19879, which adds Z-direction and yield-ratio control.
Q420C plate sizes we supply
| Form | Thickness, mm | Width, mm | Length, mm |
|---|---|---|---|
| Mill plate | 6 – 150 | 1 500 – 4 020 | 6 000 – 18 000 |
| Shanghai stock (common) | 8, 10, 12, 14, 16, 20, 25, 30, 40, 50 | 2 000 / 2 200 / 2 500 | 8 000 – 12 000 |
| Cut pieces | 6 – 150 | to drawing | to drawing |
Mill orders usually take 30 – 45 days from rolling schedule. Stock sizes can ship within a week after cutting.
Cutting and processing Q420C in our Shanghai warehouse
- Flame, plasma and CNC laser cutting to drawings; bevelling for welding
- Drilling, bending and rolling of shells
- Shot blasting Sa 2.5 and shop primer or full paint system
- Ultrasonic testing to GB/T 2970, EN 10160 or ASTM A578
Processed plates keep heat numbers traceable to the mill certificate.
How Q420C is tested and certified
Each lot carries tensile, Charpy at 0°C and chemistry results. Batches are by heat, thickness and delivery condition, up to 60 t. Optional: Z15/Z25/Z35 through-thickness to GB/T 5313, UT, product analysis, SGS/BV/TÜV witness for EN 10204 3.2.
How to order Q420C correctly
State: standard and edition (GB/T 1591-2018 Q420C), thickness × width × length, quantity, tolerance standard, any UT or Z-grade, certificate type and marking. Writing the edition avoids the most common certificate dispute we see.
Why buy Q420C from SHH STEEL
SHH STEEL works as an agent for well-known Chinese mills, so we can book rolling slots for non-stock sizes and still offer warehouse stock for urgent orders. Our team checks every certificate against GB/T 1591 before shipment. We export to Southeast Asia, the Middle East, Africa, Europe and South America, packed for sea freight with sea-worthy marking.
FAQ
-
What is Q420C steel?
- A GB/T 1591-2018 hot-rolled HSLA plate with 420 MPa minimum yield, 520 – 680 MPa tensile and 0°C impact.
-
What is the equivalent of Q420C?
- EN 10025-3 S420N and ASTM A572 Gr.60 are the usual comparisons. Neither is identical in delivery condition or impact.
-
What is the difference between Q420B and Q420C?
- Impact at 0°C instead of +20°C and P/S limited to 0.030%.
-
Is there a hot-rolled Q420D?
- Not in GB/T 1591-2018 – −20°C Q420 is ordered as Q420ND or Q420MD.
-
What is the CEV of Q420C?
- Max 0.45 (≤30 mm), 0.47 (30 – 63 mm), 0.48 (63 – 150 mm) per the heat analysis.
-
What is Q420C used for?
- High-rise columns, transmission towers, truck chassis, cranes and mining equipment.
Conclusion
Q420C is a hot-rolled 420 MPa HSLA plate grade of GB/T 1591 with 520 – 680 MPa tensile and 0°C Charpy impact. Check the thickness-dependent yield, the CEV and the product analysis tolerances when you write your purchase order.
SHH STEEL supplies Q420C mill-direct and from our Shanghai processing warehouse, with EN 10204 3.1 certificates. Related pages: Q420B, Q460C, Q420NC, EN 10025-3 S420N and our GB/T 1591 plate range. Send us your sizes for a quotation.