Q390B Steel Plate GB/T 1591 Supplier
What is Q390B steel plate?
Q390B is the entry quality of the 390 MPa class in GB/T 1591-2018 “High strength low alloy structural steels”. “Q” stands for yield strength, 390 is the minimum yield in MPa for plate up to 16 mm, and “B” means Charpy V-notch testing at +20°C. Older Chinese drawings often show 15MnV or 16MnNb for the same job; GB/T 1591-1994 merged those into Q390.
Hot-rolled Q390B is the step buyers take when Q355B is not strong enough but a quench-and-temper grade would be overkill. You save roughly 10% plate weight versus Q355B on strength-governed members, with the same welding practice.
SHH STEEL is a producer and exporter of structural plate and a sales agent for well-known Chinese mills. We keep Q390B plate in our own processing warehouse in Shanghai for cutting, drilling, shot blasting and priming. Q390B belongs to our GB/T 1591 plate range; see also our high-strength low-alloy plates overview.
Is Q390B the same as Q345B? A common mix-up
No. Q345B was the old name of what is now Q355B. Q390B is one strength class higher. If a supplier offers “Q345B/Q390B dual” plate, ask which yield value is actually guaranteed on the certificate.
Q390B specification at a glance
| Item | Q390B requirement |
|---|---|
| Standard | GB/T 1591-2018, hot-rolled (AR) condition |
| Steel type | High-strength low-alloy structural steel, killed |
| Minimum yield ReH (≤16 mm) | 390 MPa |
| Tensile strength Rm (≤100 mm) | 490 – 650 MPa |
| Impact test | KV2 ≥ 34 J at +20°C, longitudinal |
| Thickness range (SHH STEEL) | 6 – 150 mm |
| Width / length | 1 500 – 4 020 mm / 6 000 – 18 000 mm |
| Dimensions & tolerance | GB/T 709 (EN 10029 / ASTM A6 on request) |
| Certificate | EN 10204 3.1 (3.2 with third-party inspection) |
Q390B chemical composition (heat analysis)
| Element | Q390B heat analysis, % max | Role |
|---|---|---|
| C | ≤ 0.20 | strength and hardenability; kept ≤0.20 for weldability |
| Si | ≤ 0.55 | deoxidiser, adds some strength |
| Mn | ≤ 1.70 | main strengthening element; with C sets the CEV |
| P | ≤ 0.035 | impurity; lower in the tougher quality letters |
| S | ≤ 0.035 | impurity; forms MnS that hurts through-thickness and impact values |
| Nb | ≤ 0.05 | grain refiner, precipitation strengthening |
| V | ≤ 0.13 | precipitation strengthening, helps thick plate keep yield |
| Ti | ≤ 0.05 | fixes N, refines grain in the HAZ |
| Cr | ≤ 0.30 | residual / minor alloy |
| Ni | ≤ 0.50 | residual; helps low-temperature toughness |
| Cu | ≤ 0.40 | residual; limited for hot shortness |
| Mo | ≤ 0.10 | residual / minor alloy |
| N | ≤ 0.015 | kept low; free N harms toughness |
Grade B allows the widest P and S window in the family. Nb, V and Ti may be used alone or in combination; for Q390/Q420 the sum Nb+V+Ti is limited to 0.22%. Where Cu is used as a residual element the mill must report it. Values are for the ladle (heat) analysis printed on the certificate.
Product (finished plate) analysis and check tolerances for Q390B
A check analysis drilled from the finished plate may differ slightly from the ladle analysis. GB/T 1591 refers to GB/T 222 for the permitted deviations. The table applies them to the Q390B limits. The deviation applies to one side of a limit only.
| Element | Heat analysis limit, % | Permitted deviation | Product analysis limit, % |
|---|---|---|---|
| C | ≤ 0.20 | +0.02 | ≤ 0.22 |
| Si | ≤ 0.55 | +0.03 | ≤ 0.58 |
| Mn | ≤ 1.70 | +0.1 | ≤ 1.80 |
| P | ≤ 0.035 | +0.005 | ≤ 0.040 |
| S | ≤ 0.035 | +0.005 | ≤ 0.040 |
| Nb | ≤ 0.05 | +0.01 | ≤ 0.06 |
| V | ≤ 0.13 | +0.02 | ≤ 0.15 |
| Ti | ≤ 0.05 | +0.01 | ≤ 0.06 |
| Cr | ≤ 0.30 | +0.05 | ≤ 0.35 |
| Ni | ≤ 0.50 | +0.05 | ≤ 0.55 |
| Cu | ≤ 0.40 | +0.05 | ≤ 0.45 |
| Mo | ≤ 0.10 | +0.01 | ≤ 0.11 |
| N | ≤ 0.015 | +0.002 | ≤ 0.017 |
If your inspector tests a plate in a third-party lab, compare the result with the right-hand column, not with the heat analysis.
Q390B mechanical properties by thickness
| Thickness, mm | Yield ReH, MPa min | Tensile Rm, MPa | Elongation A, % min (long. / trans.) |
|---|---|---|---|
| ≤ 16 | 390 | 490 – 650 | 21 / 20 |
| > 16 – 40 | 380 | 490 – 650 | 21 / 20 |
| > 40 – 63 | 360 | 490 – 650 | 20 / 19 |
| > 63 – 100 | 340 | 490 – 650 | 20 / 19 |
| > 100 – 150 | 320 | 470 – 620 | 19 / 18 |
| Quality | Test temperature | KV2 longitudinal, J min | KV2 transverse, J min |
|---|---|---|---|
| B | +20°C | 34 | 27 |
Yield drops with thickness because thick plate cools slower and gets less rolling reduction. Design with the value for your actual thickness, not the headline 390 MPa. Impact tests use 10×10 mm specimens for plate ≥ 12 mm; thinner plate uses sub-size specimens with reduced values. Tensile tests on plate are transverse by default.
Q390B carbon equivalent (CEV) and weldability
| Thickness, mm | ≤ 30 | > 30 – 63 | > 63 – 150 | > 150 – 250 |
|---|---|---|---|---|
| CEV max, % (heat analysis) | 0.45 | 0.47 | 0.48 | — |
CEV = C + Mn/6 + (Cr+Mo+V)/5 + (Ni+Cu)/15. Real heats from our mills usually come in around 0.40 – 0.44 on 20 – 40 mm plate. Q390 plate welds with standard E50/E55-class consumables (AWS E7018 / E8018 type, ER50-6 / ER55 wire). Preheat of 50 – 100°C is common above 25 mm or in restrained joints; low-hydrogen practice is the key point.
Q390B equivalent grades: EN, ASTM, JIS
| System | Grade | Comment |
|---|---|---|
| ASTM | ASTM A572 Gr.55 | 380 MPa min yield, no impact by default |
| JIS | JIS G3106 SM520B | 355 MPa yield (≤16 mm), 0°C impact |
| EN 10025-3 | EN 10025-3 S420N (closest) | Normalized 420 MPa fine-grain; EN 10025-2 has no S390 grade |
| GB/T 1591-2018 | Q390NB | Normalized version, same strength |
“Equivalent” means similar, not identical. Strength classes, impact temperatures and delivery conditions differ between standards. A plate can be dual-certified only if one heat meets both books in full; ask us before you assume it.
Q390B vs Q355B vs Q420B: which one to choose?
| Grade | Yield ≤16 mm, MPa | Tensile ≤100 mm, MPa | Impact |
|---|---|---|---|
| Q355B | 355 | 470 – 630 | +20°C |
| Q390B | 390 | 490 – 650 | +20°C |
| Q420B | 420 | 520 – 680 | +20°C |
Q355B vs Q390B: same +20°C test, but 355 versus 390 MPa yield and a lower CEV. Q420B adds another 30 MPa. Many buyers search “Q390B vs Q345B” because Q345B was renamed Q355B in 2018.
Where is Q390B used?
Q390B plate is used for building frames, mezzanines, steel bridges for indoor service, truck bodies, excavator booms, storage tanks supports, general fabricated structures.
For building columns with through-thickness loads, compare with Q390GJC building plate to GB/T 19879, which adds Z-direction and yield-ratio control.
Q390B plate sizes we supply
| Form | Thickness, mm | Width, mm | Length, mm |
|---|---|---|---|
| Mill plate | 6 – 150 | 1 500 – 4 020 | 6 000 – 18 000 |
| Shanghai stock (common) | 8, 10, 12, 14, 16, 20, 25, 30, 40, 50 | 2 000 / 2 200 / 2 500 | 8 000 – 12 000 |
| Cut pieces | 6 – 150 | to drawing | to drawing |
Mill orders usually take 30 – 45 days from rolling schedule. Stock sizes can ship within a week after cutting.
Cutting and processing Q390B in our Shanghai warehouse
- Flame, plasma and CNC laser cutting to drawings; bevelling for welding
- Drilling, bending and rolling of shells
- Shot blasting Sa 2.5 and shop primer or full paint system
- Ultrasonic testing to GB/T 2970, EN 10160 or ASTM A578
Processed plates keep heat numbers traceable to the mill certificate.
How Q390B is tested and certified
Each lot carries tensile, Charpy at +20°C and chemistry results. Batches are by heat, thickness and delivery condition, up to 60 t. Optional: Z15/Z25/Z35 through-thickness to GB/T 5313, UT, product analysis, SGS/BV/TÜV witness for EN 10204 3.2.
How to order Q390B correctly
State: standard and edition (GB/T 1591-2018 Q390B), thickness × width × length, quantity, tolerance standard, any UT or Z-grade, certificate type and marking. Writing the edition avoids the most common certificate dispute we see.
Why buy Q390B from SHH STEEL
SHH STEEL works as an agent for well-known Chinese mills, so we can book rolling slots for non-stock sizes and still offer warehouse stock for urgent orders. Our team checks every certificate against GB/T 1591 before shipment. We export to Southeast Asia, the Middle East, Africa, Europe and South America, packed for sea freight with sea-worthy marking.
FAQ
-
What is Q390B steel equivalent to?
- The closest comparisons are ASTM A572 Gr.55 and JIS G3106 SM520B. The nearest EN comparison is EN 10025-3 S420N; EN 10025-2 has no S390 grade.
-
What is the yield strength of Q390B?
- Minimum 390 MPa up to 16 mm, 380 MPa for 16 – 40 mm, 360 MPa for 40 – 63 mm, 340 MPa for 63 – 100 mm and 320 MPa for 100 – 150 mm (GB/T 1591-2018).
-
What is the difference between Q355B and Q390B?
- Q390B has 35 MPa higher yield and 490 – 650 MPa tensile (vs 470 – 630). Both are impact-tested at +20°C.
-
What does the B in Q390B mean?
- B is the quality grade: Charpy V impact ≥ 34 J at +20°C, longitudinal.
-
Is Q390B weldable?
- Yes. CEV is max 0.45 up to 30 mm; use low-hydrogen consumables and preheat thick or restrained joints.
-
What was Q390B called before?
- Older Chinese standards used 15MnV, 15MnTi and 16MnNb for this strength level.
Conclusion
Q390B is a hot-rolled 390 MPa HSLA plate grade of GB/T 1591 with 490 – 650 MPa tensile and +20°C Charpy impact. Check the thickness-dependent yield, the CEV and the product analysis tolerances when you write your purchase order.
SHH STEEL supplies Q390B mill-direct and from our Shanghai processing warehouse, with EN 10204 3.1 certificates. Related pages: Q355B, Q420B, Q390NB, EN 10025-3 S420N and our GB/T 1591 plate range. Send us your sizes for a quotation.