GB/T 19879 Q345GJE Building Steel Plate Supplier

GB/T 19879 Q345GJE, renamed Q355GJE in the 2023 edition, is building structure steel plate with a capped yield window, yield ratio ≤0.80 (2015) or ≤0.83 (2023) and 47 J at −40°C. SHH STEEL supplies it 6–200 mm, mill-direct, to either edition, with Z15–Z35 and heat and product analysis.
Keywords
Q345GJE, Q345GJE steel plate, GB/T 19879 Q345GJE, Q345GJ-E, Q355GJE, Q345GJE vs Q355GJE, Q345GJEZ15, Q345GJEZ25, Q345GJEZ35, Q345GJ, building structure steel plate, Q345GJE supplier
Equivalent Grades
Equivalent Grades: GB/T 19879-2015 Q345GJE = GB/T 19879-2023 Q355GJE / JIS G3136 SN490C (closest building steel) / EN 10025-3 S355NL (strength only) / ASTM A572 Gr.50 / JIS G3106 SM490 — Material Specification: GB/T 19879-2015 (superseded by GB/T 19879-2023) — Delivery: AR, CR, NR, N or TMCP; −40°C impact
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Q345GJE vs Q355NE
Q345GJ vs Q355GJ
Material Comparison
Z15 / Z25 / Z35
Equivalent Material Grades
Weldability
Heat Treatment and Delivery Condition
Dimensions
Tolerances
Supplementary Requirements
Price and Ordering
Applications
Supply Capability
Why Choose SHH STEEL
FAQ
Conclusion

What is GB/T 19879 Q345GJE Building Steel Plate?

Q345GJE, also written Q345GJ-E or Q345 GJE, is hot-rolled steel plate for building structures under GB/T 19879-2015. Q means yield, 345 is the minimum yield in MPa, GJ (gao jian) marks high-performance building steel, and E is the quality grade: Charpy V-notch at −40°C, at least 47 J. The 2023 edition of the standard calls the same steel Q355GJE.

The GJ rules are what the structural engineer is paying for. Q345GJE sets a maximum yield as well as a minimum, caps the yield ratio, limits carbon equivalent by thickness and delivery route, and keeps P and S low. The frame then yields where the designer expects.

Q345GJE is the −40°C member of the family. It fits exposed steel in the coldest parts of northern China and export work in Central Asia, Russia or Mongolia, where the design temperature falls below what D-grade plate is tested for.

GB/T 19879-2023 replaced GB/T 19879-2015 on 1 April 2024. GB/T 19879-2023 renamed Q345GJ to Q355GJ. Minimum yield rose from 345 to 355 MPa, the yield window widened from 110 MPa (345–455) to 120 MPa (355–475), the yield-ratio cap moved from 0.80 to 0.83, and CEV for plate up to 50 mm moved from 0.42% to 0.43%. Chemistry did not change. Sister grades are listed under GB/T 19879, including Q345GJB.

SHH STEEL (Shanghai Shenghonghe Import & Export Co., Ltd.) is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. We ship Q345GJE cut to size with an EN 10204 3.1 or 3.2 certificate.

Material Specification

Specification element Requirement SHH STEEL compliance
Plate standard GB/T 19879-2015 Q345GJE, or GB/T 19879-2023 Q355GJE Confirmed
Thickness for Q345GJ 6 mm – 200 mm Confirmed
Yield strength 345 MPa min; 345–455 MPa 16–50 mm (2015) / 355–475 MPa 16–100 mm (2023) Confirmed
Tensile strength 490 – 610 MPa (to 100 mm) Confirmed
Yield ratio ≤ 0.80 (2015) / ≤ 0.83 (2023) Printed on MTC
Quality grade E, Charpy V at −40°C, KV2 ≥ 47 J, longitudinal Confirmed
Delivery condition AR, CR, NR, N or TMCP As ordered
Through-thickness Z15, Z25 or Z35 to GB/T 5313 As ordered
Dimensions GB/T 709-2019, thickness tolerance Class B Confirmed
Chemistry report Heat analysis + CEV; product analysis on request Confirmed
Certificate EN 10204 3.1 or 3.2 As ordered

Grades often confused with it are GB/T 1591 Q355NE, EN 10025-3 S355NL and ASTM A572 Gr.50. None of them carries the GJ yield cap or yield-ratio rule.

Chemical Composition: Heat Analysis and Product Analysis

GB/T 19879 controls chemistry twice. The heat (ladle) analysis is taken from the melt and must meet Table 1 of the standard. The product analysis is taken from the finished plate and may sit slightly outside Table 1, by the permitted deviations of GB/T 222 (clause 7.1.4). Both are valid acceptance checks, but they are not the same number.

Table 1 below is the heat analysis for Q345GJE. The columns on the right show the quality-grade groups at Q345GJ.

Table 1. Heat (ladle) analysis, GB/T 19879-2023 Table 1, %

Element Q345GJE heat analysis (%) Q345GJ B / C Q345GJ D / E
C, max 0.18 0.20 0.18
Si, max 0.55 0.55 0.55
Mn, max 1.60 1.60 1.60
P, max 0.020 0.025 0.020
S, max 0.010 0.015 0.010
V, max 0.150 0.150 0.150
Nb, max 0.070 0.070 0.070
Ti, max 0.035 0.035 0.035
Als, min 0.015 0.015 0.015
Cr, max 0.30 0.30 0.30
Cu, max 0.30 0.30 0.30
Ni, max 0.30 0.30 0.30
Mo, max 0.20 0.20 0.20
V + Nb + Ti, max (if combined) 0.15 0.15 0.15

Notes to Table 1. Total aluminium (Alt ≥ 0.020%) may replace acid-soluble aluminium. If Al, V, Nb or Ti is added alone or together at 0.015% or more, the minimum aluminium does not apply. V + Nb + Ti, when combined, is limited to 0.15%. These limits are the same in the 2015 and 2023 editions.

B and C grades share one chemistry column. D and E grades tighten carbon to 0.18%, phosphorus to 0.020% and sulfur to 0.010%, because they are tested at −20°C and −40°C.

Table 2. Product analysis limits for Q345GJE, GB/T 19879 clause 7.1.4 with GB/T 222-2025, %

Element Heat limit (%) Permitted deviation, GB/T 222-2025 Table 1 Q345GJE product analysis limit (%)
C ≤ 0.18 +0.02 ≤ 0.20
Si ≤ 0.55 +0.05 ≤ 0.60
Mn ≤ 1.60 +0.06 ≤ 1.66
P ≤ 0.020 +0.005 ≤ 0.025
S ≤ 0.010 +0.005 ≤ 0.015
V ≤ 0.150 +0.02 ≤ 0.170
Nb ≤ 0.070 ±0.005 ≤ 0.075 (Table 1 lists Nb to 0.060%; agree above that)
Ti ≤ 0.035 +0.02 ≤ 0.055
Als ≥ 0.015 −0.003 ≥ 0.012
Cr ≤ 0.30 +0.05 ≤ 0.35
Cu ≤ 0.30 +0.05 ≤ 0.35
Ni ≤ 0.30 +0.05 ≤ 0.35
Mo ≤ 0.20 Not listed in Table 1 Agree in contract (alloy-steel Table 2 would give ≤ 0.21)

How to read Table 2. The band is chosen by the Table 1 upper limit. Si ≤0.55% is above 0.37%, so +0.05% applies; Mn ≤1.60% falls in the 0.80–1.70% band, so +0.06%. For one heat an element may deviate in one direction only.

GB/T 222-2025 replaced GB/T 222-2006 on 1 December 2025. One more rule from it matters to buyers: if no reliable heat analysis exists, the product analysis must meet the heat limits with no deviation at all (clause 5.6).

Z-grade plate is cleaner still. GB/T 5313-2023 limits sulfur by heat analysis:

Z grade Heat sulfur, max (%) Reduction of area, avg / single (%)
Z15 0.010 15 / 10
Z25 0.007 25 / 15
Z35 0.005 35 / 25

CEV and Pcm are always worked out from the heat analysis, not the product analysis. SHH STEEL prints the heat values used and adds a product-analysis column on request. This is building steel, not boiler chemistry such as GB/T 713 Q345R in GB/T 713.

Mechanical Properties

Values below follow Table 3 and Table 5 of GB/T 19879-2023 for Q355GJ, the 2023 name of Q345GJ. Tensile specimens are transverse; Charpy specimens are longitudinal.

Thickness Upper yield ReH (MPa) Tensile Rm (MPa) Yield ratio, max Elongation A, min
6 – 16 mm ≥ 355 490 – 610 0.83 22%
> 16 – 100 mm 355 – 475 490 – 610 0.83 22%
> 100 – 150 mm 335 – 455 470 – 600 0.83 22%
> 150 – 200 mm 325 – 445 470 – 600 0.83 22%

For orders to the 2015 edition, Q345GJ uses lower yield ReL and these bands, with yield ratio ≤ 0.80 and A ≥ 22%:

Thickness (2015) ReL (MPa) Rm (MPa)
6 – 16 mm ≥ 345 490 – 610
> 16 – 50 mm 345 – 455 490 – 610
> 50 – 100 mm 335 – 445 490 – 610
> 100 – 150 mm 325 – 435 470 – 610
> 150 – 200 mm 305 – 415 470 – 610
Test Q345GJE requirement
Charpy V-notch, longitudinal −40°C, KV2 ≥ 47 J, average of 3
Single value One value may fall below the average requirement, not below 70% of it (GB/T 17505)
Sub-size specimens 7.5 mm or 5 mm wide when plate is too thin: 75% or 50% of the required energy
180° bend Per Table 6 to GB/T 232; may be omitted when the mill guarantees it (7.4.3.2)
Through-thickness (≥ 15 mm) Z15, Z25 or Z35 to GB/T 5313, when ordered

Density for theoretical weight is 7.85 g/cm³.

Q345GJE vs Q355NE and Q345E: Building Plate or General Structural Plate?

Q345E was the GB/T 1591-2008 name. GB/T 1591-2018 replaced it with GB/T 1591 Q355NE. Q345GJE is a different book again: GB/T 19879, written for building frames. Buyers mix the three up every week.

The general structural grade is sold on its minimum yield. The building grade is sold on control: a yield ceiling, a yield-ratio cap, a CEV limit, lower P and S, and 47 J impact. In a seismic frame those rules decide where the steel yields first.

Property Q355NE (GB/T 1591-2018) Q345GJE (GB/T 19879-2015) Q355GJE (GB/T 19879-2023)
Yield at 16 mm 355 MPa 345 MPa 355 MPa
Yield at 40–63 mm 335 MPa min 345–455 MPa (to 50 mm) 355–475 MPa
Yield at 80–100 mm 315 MPa min 335–445 MPa 355–475 MPa
Yield upper limit None Yes (110 MPa window) Yes (120 MPa window)
Yield ratio No limit ≤ 0.80 ≤ 0.83
Tensile, to 100 mm 470 – 630 MPa 490 – 610 MPa 490 – 610 MPa
Impact −40°C, lower energy than 47 J −40°C, 47 J −40°C, 47 J
P / S, max Per GB/T 1591 grade 0.020 / 0.010% 0.020 / 0.010%
Maximum thickness 250 mm (AR tables) 200 mm 200 mm

Q345GJE can replace Q355NE in almost every case. Q355NE cannot replace Q345GJE: its certificate never reports a yield ratio or a GJ CEV band.

GB/T 1591-2018 places −40°C at 355 MPa in the N and M routes (GB/T 1591 Q355NE, GB/T 1591 Q355ME). EN 10025-3 S355NL and EN 10025-4 S355ML are tested at −50°C. None of them caps yield.

Q345GJE vs Q355GJE: What Changed in GB/T 19879-2023

GB/T 19879-2023 replaced the 2015 edition on 1 April 2024 and renamed Q345GJ to Q355GJ. Chemistry is identical. Strength and ratio rules are not, and that is what decides whether one certificate can serve both names.

Rule Q345GJE (2015) Q355GJE (2023)
Yield measured as Lower yield ReL Upper yield ReH
6 – 16 mm ≥ 345 MPa ≥ 355 MPa
> 16 – 50 mm 345 – 455 MPa 355 – 475 MPa
> 50 – 100 mm 335 – 445 MPa 355 – 475 MPa
> 100 – 150 mm 325 – 435 MPa 335 – 455 MPa
> 150 – 200 mm 305 – 415 MPa 325 – 445 MPa
Tensile, to 100 mm 490 – 610 MPa 490 – 610 MPa
Yield ratio ≤ 0.80 ≤ 0.83
CEV ≤ 50 mm (AR/CR/N) 0.42% 0.43%
Impact −40°C, 47 J −40°C, 47 J
Delivery codes WAR, WCR, N, TMCP AR, CR, NR, N, TMCP

The trap is the overlap. A Q355GJ plate at 470 MPa yield or a 0.82 ratio passes 2023 but fails a 2015 Q345GJ order. A Q345GJ plate at 350 MPa passes 2015 but fails 2023.

When a drawing still says Q345GJE, we ask which edition the reviewer will use. If both, we dual-certify only plate that sits inside both windows: 355–455 MPa yield (to 50 mm) and a ratio of 0.80 or lower.

Q345GJB, Q345GJC, Q345GJD or Q345GJE: Which Quality Grade?

Grade Impact temperature Energy, min C / P / S max (%) Typical use
Q345GJB +20°C 47 J 0.20 / 0.025 / 0.015 Heated interiors, mild climates
Q345GJC 0°C 47 J 0.20 / 0.025 / 0.015 Cold regions, exposed frames
Q345GJD −20°C 47 J 0.18 / 0.020 / 0.010 Severe winters, thick welded nodes
Q345GJE −40°C 47 J 0.18 / 0.020 / 0.010 Arctic and low-temperature sites

Strength, yield ratio and CEV do not change from B to E. Only the impact temperature and the D/E chemistry move. Pick the letter from the lowest service or erection temperature.

Q345GJE is the coldest letter in GB/T 19879; there is no F grade in this standard. For the same letter at another strength level: one level up, Q390GJE; one level down, Q235GJE.

Q345GJEZ15, Q345GJEZ25 and Q345GJEZ35: Through-Thickness Plate

Thick plate loaded across its thickness can tear in layers under weld shrinkage. Column flanges at beam-flange welds, diaphragm plates in box columns and base plates under heavy tension are the usual places. A Z grade guarantees ductility in that direction.

The designation adds the Z level to the grade, for example Q345GJEZ25. Z tests apply to plate 15 mm and thicker and follow GB/T 5313-2023.

Z grade Heat sulfur, max (%) Reduction of area, avg / single (%)
Z15 0.010 15 / 10
Z25 0.007 25 / 15
Z35 0.005 35 / 25

The E melt already caps S at 0.010%, the Z15 limit, so Z25 and Z35 are the levels that change the steelmaking.

GB/T 19879-2023 clause 7.6 requires every Z plate to be ultrasonic tested one by one to GB/T 2970, acceptance level III. Z35 costs most: lowest sulfur, more rejects, and a Z test on each plate.

Ask for Z only where the joint needs it. Over-specifying Z35 across a whole order adds cost and lead time without helping the frame.

Equivalent Material Grades

The nearest foreign building steel is JIS G3136 SN490, which also caps yield and yield ratio. ASTM A992 is the US seismic shape grade with a 0.85 ratio cap; it is a section standard, not plate.

Designation Region Standard Notes
Q345GJE China GB/T 19879-2015 Grade on this page
Q355GJE China GB/T 19879-2023 Current name; see the 2015/2023 table
SN490C Japan JIS G3136 Closest building steel: yield range, ratio ≤ 0.80, Z option
EN 10025-3 S355NL Europe EN 10025-3 Strength and temperature comparison only
EN 10025-2 S355K2 Europe EN 10025-2 40 J / 27 J at −20°C
JIS G3106 SM490C Japan JIS G3106 No yield-ratio rule
ASTM A572 Gr.50 USA ASTM A572 345 MPa; no impact or ratio rule
ASTM A709 Grade 50 USA ASTM A709 Bridge grade; toughness by zone
DIN 17100 St52-3 Germany DIN 17100 (withdrawn) Legacy name

For plate certificates on EN projects, EN 10025-2 or EN 10025-3 plate with EN 10164 Z grades is the usual route. We dual-certify only when both books pass, and say so on the MTC.

Weldability

GB/T 19879 makes the mill calculate CEV from the heat analysis and print it, together with the elements used, on every Q345GJE certificate:

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15

Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B

Delivery condition CEV ≤ 50 mm CEV > 50 – 100 mm CEV > 100 – 150 mm CEV > 150 – 200 mm Pcm ≤ 50 mm Pcm > 50 – 100 mm Pcm > 100 – 150 mm Pcm > 150 – 200 mm
AR, CR, NR, N (2023) 0.43 0.45 0.46 0.47 0.26 0.29 0.30 0.30
TMCP (2023) 0.38 0.40 By agreement — 0.24 0.26 — —
WAR, WCR, N (2015, Q345GJ) 0.42 0.44 0.46 0.47 — — — —

At 0.43% CEV (2023, ≤50 mm) Q355GJ welds with ordinary structural procedures. Preheat climbs with thickness and restraint; plate over 50 mm in box columns is where most shops start preheating as routine.

The E letter helps: carbon is capped at 0.18% and P and S are lower, which reduces hot-cracking and HAZ embrittlement risk.

Typical consumables: E50-class low-hydrogen electrodes (E5015/E5016) or ER50-6 wire; AWS E7018 / ER70S-6. Shops work to GB 50661 or AWS D1.1. Write the CEV basis (actual heat, not table maximum) into the WPS.

Heat Treatment and Delivery Condition

Q345GJE/Q355GJE may be delivered AR, CR, NR or N, or TMCP. In the 2015 text the codes were WAR (hot rolled), WCR (controlled rolled), N and TMCP.

Up to about 60 mm most plate ships CR or TMCP. Thick column plate and Z35 plate often ship normalized, which evens out properties through the thickness.

The GB/T 1591 grades with fixed delivery routes are GB/T 1591 Q355ND (normalized) and GB/T 1591 Q355MD (TMCP); compare with EN 10025-3 S355N and EN 10025-4 S355M in Europe.

Test lots follow clause 9.2 of GB/T 19879-2023; retests and judgement follow GB/T 17505.

Dimensions

Usual Q345GJE supply range from SHH STEEL:

  • Thickness: 6 mm – 200 mm; most orders 10 mm – 120 mm
  • Width: 1500 mm – 3000 mm standard; wider by mill confirmation
  • Length: 3000 mm – 12000 mm; longer by enquiry
  • Edge: mill edge or cut edge
  • Weight: theoretical, on the mean of maximum and minimum thickness, 7.85 g/cm³

Column flanges, diaphragms, stiffeners and gussets are cut to drawing. Rolled sections for the same frame are under steel beam profiles and steel structural profiles.

Tolerances

GB/T 19879-2023 sends dimensions and shape to GB/T 709-2019. Thickness tolerance is Class B by default: fixed minus 0.30 mm, plus by thickness and width. Class C (zero minus) is available by agreement.

Nominal thickness (mm) Width ≤ 1500 mm Width > 1500 – 2500 mm
> 8 – 15 −0.30 / +0.80 −0.30 / +1.00
> 15 – 25 −0.30 / +1.00 −0.30 / +1.20
> 25 – 40 −0.30 / +1.10 −0.30 / +1.30
> 40 – 60 −0.30 / +1.30 −0.30 / +1.50
> 60 – 100 −0.30 / +1.50 −0.30 / +1.80
> 100 – 150 −0.30 / +2.10 −0.30 / +2.50

Plate over 150 mm follows the heavier rows of GB/T 709; we state the figures on the offer. Flatness and width follow GB/T 709. EN 10029 or ASTM A6 tolerances are possible if written on the order.

Supplementary Requirements

Q345GJE already fixes strength, yield ratio, CEV and −40°C impact. Anything more goes on the purchase order.

  • Edition: GB/T 19879-2015 (Q345GJ) or -2023 (Q355GJ). Never write only Q345.
  • Product analysis: ask for a second chemistry column checked to GB/T 222.
  • Through-thickness: add Z15, Z25 or Z35, e.g. Q345GJEZ25.
  • Delivery condition: name it (AR, CR, NR, N or TMCP) if the welding procedure depends on it.
  • Ultrasonic testing beyond Z plates: GB/T 2970 class, or EN 10160 / ASTM A578.
  • Impact: extra test positions (e.g. quarter thickness) or transverse tests, if the owner wants them beyond the E letter.
  • Tolerance: Class C for zero minus.
  • Inspection: EN 10204 3.2 with SGS, BV, TÜV or a named inspector.

Q345GJE Price Factors and How to Order

A Q345GJE price per ton is a base price plus extras. The extras explain most gaps between quotes.

Cost driver Effect on price
GJ grade over general Q345 plate Grade extra for cleaner steel, yield control and CEV
Quality letter E Highest letter extra: −40°C testing, cleaner melt, more retest risk
Delivery route N and TMCP carry extras over AR/CR
Thickness Thin and very thick plate carry size extras; 10–60 mm is usually cheapest
Z15 / Z25 / Z35 Desulfurization, plate-by-plate Z test and UT; Z35 costs most
Width and length Over 3000 mm wide or 12 m long needs mill confirmation
Quantity per size Mill rolling minimums per size; small lots come from stock or combined rolling
Inspection and cutting 3.2 witness, profile cutting, blasting and priming are quoted per item

To get a firm quote in one round, send:

  • Grade and edition, e.g. Q345GJEZ25 to GB/T 19879-2015
  • Thickness × width × length and pieces or tonnes
  • Delivery route, UT standard and class
  • Certificate type and inspector
  • Destination port and Incoterm

We quote plate price, extras and freight line by line, so you can compare like with like. Need a different letter? See Q345GJD.

Applications

Sector Typical Q345GJE components
High-rise towers Box and H column plates, transfer girders, outrigger webs
Airports and stadiums Long-span roof trusses, tree columns, node plates
Seismic frames Beam-to-column panel zones, links, brace gussets
Industrial buildings Heavy crane girders, column bases
Bridges in buildings Skybridges, podium transfer trusses

E grade is for the coldest sites and for owners who specify −40°C for every primary member.

It is the wrong plate for pressure equipment (pressure vessel steel plates), for bare exposed steel (weathering steel plates) or for ship hulls (shipbuilding steel plates).

Supply Capability and Global Delivery

SHH STEEL sources Q345GJE from first-line building-steel mills: Wuyang (Wugang), a drafting mill of GB/T 19879, plus Xinyu, Valin Xiangtan, Shougang, Puyang and Hongchang when size requires.

  • Certificates: EN 10204 3.1 standard; 3.2 with third-party witness
  • Tests: tensile, −40°C Charpy, bend, Z test to GB/T 5313, UT to GB/T 2970, product analysis
  • Processing: CNC plasma and flame cutting, bevelling, drilling, shot blast and primer
  • Terms: FOB Shanghai, CFR, CIF; TT, LC or TT + LC
  • Marking: steel-stamped and paint-marked with grade, heat, size and mill

We ship GB, ASTM, ASME, EN, DIN and JIS plate to the United States, Europe, the Middle East, Southeast Asia, Africa and South America. Q345GJE mostly goes to EPC contractors building Chinese-code projects abroad.

Lead time: stock sizes about 5–7 days; mill rolling about 30–45 days; Z35 or 3.2 inspection adds about 1–2 weeks. Sea time from Shanghai is about 7–12 days to Singapore and 28–35 days to Rotterdam.

Why Choose SHH STEEL

SHH STEEL is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. For Q345GJE that means real GJ plate at mill price, not relabelled general structural plate.

Before shipment we check four lines on every certificate: yield inside the GJ window, yield ratio within the cap, CEV inside the thickness band for the delivery route, and −40°C impact at 47 J or more. If one fails, the plate does not ship as GJ.

We also tell buyers when they are over-specifying. If the member is outside the lateral system, GB/T 1591 Q355D may be enough, and we will tell you. Browse more structural steel plates and high strength low alloy plates.

FAQ

What is Q345GJE steel?
Q345GJE is building structure steel plate to GB/T 19879-2015 with 345 MPa minimum yield, a 110 MPa yield window, yield ratio ≤0.80, CEV limits and Charpy impact of at least 47 J at −40°C. GB/T 19879-2023 renamed it Q355GJE, with 355–475 MPa yield and a 0.83 ratio cap.
What is the difference between Q345GJE and Q355NE?
Q355NE is general structural plate to GB/T 1591-2018 with a minimum yield that falls with thickness and no yield cap or ratio limit. Q345GJE is building plate to GB/T 19879 with a capped yield window, a yield ratio of 0.80 (2015) or 0.83 (Q355GJE, 2023), CEV limits and 47 J at −40°C. Q345GJE can replace Q355NE; the reverse needs designer approval.
Is Q345GJE suitable for −40°C service?
Yes. Q345GJE is Charpy tested at −40°C and must average at least 47 J on longitudinal specimens. GB/T 19879 has no colder letter, so for design temperatures below −40°C look at GB/T 1591 Q355MF or EN S355ML (−50°C) and check the yield-cap rules separately.
What thickness range does Q345GJ cover?
Q345GJ covers 6 mm to 200 mm in GB/T 19879-2015, and Q355GJ keeps 6–200 mm in the 2023 edition. It is the only GJ strength level that goes to 200 mm; Q235GJ and Q390GJ–Q460GJ stop at 150 mm.
What certificate comes with Q345GJE plate?
Q345GJE ships with an EN 10204 3.1 mill certificate by default, or 3.2 with third-party witness. It shows heat analysis and the elements used for CEV, yield, tensile, yield ratio, elongation, Charpy at −40°C, delivery condition, and Z and UT results when ordered.
What is the ASTM or EN equivalent of Q345GJE?
The current Chinese name is Q355GJE (GB/T 19879-2023). Abroad, the closest building steel is JIS G3136 SN490C. EN 10025-3 S355NL and ASTM A572 Gr.50 match strength only: they have no yield cap or yield-ratio limit, so they are not direct substitutes.

Conclusion

Q345GJE steel plate to GB/T 19879 is building structure plate with 345 MPa (2015) or 355 MPa (2023, as Q355GJE) minimum yield, a capped yield window, a yield-ratio limit and 47 J impact at −40°C. It shares its chemistry with Q345GJB but proves toughness at its own letter. It is not general structural plate under GB/T 1591.

SHH STEEL supplies Q345GJE with heat analysis, CEV, yield ratio and impact on an EN 10204 3.1 or 3.2 certificate, and adds a product analysis checked to GB/T 222 when you need it. Z15, Z25 or Z35, UT to GB/T 2970, Class B or C tolerance, cutting and blasting are available.

We ship from Shanghai to buyers worldwide. Browse the full GB/T 19879 range or other carbon steel plates.

Send the edition, quality letter, Z level and size list; we confirm mill, delivery route, lead time and price in one reply. Contact SHH STEEL for a mill-direct quotation on Q345GJE building steel plate.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X