Close view of GB/T 19879 Q345GJB building steel plate stack edges at SHH STEEL

GB/T 19879 Q345GJB Building Steel Plate Supplier

GB/T 19879 Q345GJB, renamed Q355GJB in the 2023 edition, is building structure steel plate with a capped yield window, yield ratio ≤0.80 (2015) or ≤0.83 (2023) and 47 J at +20°C. SHH STEEL supplies it 6–200 mm, mill-direct, to either edition, with Z15–Z35 and heat and product analysis.
Keywords
Q345GJB, Q345GJB steel plate, GB/T 19879 Q345GJB, Q345GJ-B, Q355GJB, Q345GJB vs Q355GJB, Q345GJBZ15, Q345GJBZ25, Q345GJBZ35, Q345GJ, building structure steel plate, Q345GJB supplier
Equivalent Grades:
GB/T 19879-2015 Q345GJB = GB/T 19879-2023 Q355GJB / JIS G3136 SN490B (closest building steel) / EN 10025-2 S355JR (strength only) / ASTM A572 Gr.50 / JIS G3106 SM490 — Material Specification: GB/T 19879-2015 (superseded by GB/T 19879-2023) — Delivery: AR, CR, NR, N or TMCP; +20°C impact
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Q345GJB vs Q355B
Q345GJ vs Q355GJ
Material Comparison
Z15 / Z25 / Z35
Equivalent Material Grades
Weldability
Heat Treatment and Delivery Condition
Dimensions
Tolerances
Supplementary Requirements
Price and Ordering
Applications
Supply Capability
Why Choose SHH STEEL
FAQ
Conclusion

What is GB/T 19879 Q345GJB Building Steel Plate?

Q345GJB, also written Q345GJ-B or Q345 GJB, is hot-rolled steel plate for building structures under GB/T 19879-2015. Q means yield, 345 is the minimum yield in MPa, GJ (gao jian) marks high-performance building steel, and B is the quality grade: Charpy V-notch at +20°C, at least 47 J. The 2023 edition of the standard calls the same steel Q355GJB.

The GJ rules are what the structural engineer is paying for. Q345GJB sets a maximum yield as well as a minimum, caps the yield ratio, limits carbon equivalent by thickness and delivery route, and keeps P and S low. The frame then yields where the designer expects.

Q345GJB is the most quoted name in older Chinese building specifications, and the one most likely to cause a certificate dispute today. Under GB/T 19879-2023 the grade is Q355GJB: same family, but a higher minimum yield, a wider yield window and a looser yield ratio. B means +20°C impact, so it suits heated interiors.

GB/T 19879-2023 replaced GB/T 19879-2015 on 1 April 2024. GB/T 19879-2023 renamed Q345GJ to Q355GJ. Minimum yield rose from 345 to 355 MPa, the yield window widened from 110 MPa (345–455) to 120 MPa (355–475), the yield-ratio cap moved from 0.80 to 0.83, and CEV for plate up to 50 mm moved from 0.42% to 0.43%. Chemistry did not change. Sister grades are listed under GB/T 19879, including Q345GJC.

SHH STEEL (Shanghai Shenghonghe Import & Export Co., Ltd.) is a steel manufacturer and exporter and global steel mill sourcing partner, mill-direct, China origin. We ship Q345GJB cut to size with an EN 10204 3.1 or 3.2 certificate.

Material Specification

Specification element Requirement SHH STEEL compliance
Plate standard GB/T 19879-2015 Q345GJB, or GB/T 19879-2023 Q355GJB Confirmed
Thickness for Q345GJ 6 mm – 200 mm Confirmed
Yield strength 345 MPa min; 345–455 MPa 16–50 mm (2015) / 355–475 MPa 16–100 mm (2023) Confirmed
Tensile strength 490 – 610 MPa (to 100 mm) Confirmed
Yield ratio ≤ 0.80 (2015) / ≤ 0.83 (2023) Printed on MTC
Quality grade B, Charpy V at +20°C, KV2 ≥ 47 J, longitudinal Confirmed
Delivery condition AR, CR, NR, N or TMCP As ordered
Through-thickness Z15, Z25 or Z35 to GB/T 5313 As ordered
Dimensions GB/T 709-2019, thickness tolerance Class B Confirmed
Chemistry report Heat analysis + CEV; product analysis on request Confirmed
Certificate EN 10204 3.1 or 3.2 As ordered

Grades often confused with it are GB/T 1591 Q355B, EN 10025-2 S355JR and ASTM A572 Gr.50. None of them carries the GJ yield cap or yield-ratio rule.

Chemical Composition: Heat Analysis and Product Analysis

Two chemistry numbers exist for every Q345GJB plate. The mill reports the heat (ladle) analysis, which must sit inside Table 1. A check analysis drilled from the plate is the product analysis; clause 7.1.4 of GB/T 19879 lets it differ from Table 1 by the GB/T 222 deviations.

Table 1 below is the heat analysis for Q345GJB. The columns on the right show the quality-grade groups at Q345GJ.

Table 1. Heat (ladle) analysis, GB/T 19879-2023 Table 1, %

Element Q345GJB heat analysis (%) Q345GJ B / C Q345GJ D / E
C, max 0.20 0.20 0.18
Si, max 0.55 0.55 0.55
Mn, max 1.60 1.60 1.60
P, max 0.025 0.025 0.020
S, max 0.015 0.015 0.010
V, max 0.150 0.150 0.150
Nb, max 0.070 0.070 0.070
Ti, max 0.035 0.035 0.035
Als, min 0.015 0.015 0.015
Cr, max 0.30 0.30 0.30
Cu, max 0.30 0.30 0.30
Ni, max 0.30 0.30 0.30
Mo, max 0.20 0.20 0.20
V + Nb + Ti, max (if combined) 0.15 0.15 0.15

Notes to Table 1. Total aluminium (Alt ≥ 0.020%) may replace acid-soluble aluminium. If Al, V, Nb or Ti is added alone or together at 0.015% or more, the minimum aluminium does not apply. V + Nb + Ti, when combined, is limited to 0.15%. These limits are the same in the 2015 and 2023 editions.

B and C grades share one chemistry column. D and E grades tighten carbon to 0.18%, phosphorus to 0.020% and sulfur to 0.010%, because they are tested at −20°C and −40°C.

Table 2. Product analysis limits for Q345GJB, GB/T 19879 clause 7.1.4 with GB/T 222-2025, %

Element Heat limit (%) Permitted deviation, GB/T 222-2025 Table 1 Q345GJB product analysis limit (%)
C ≤ 0.20 +0.02 ≤ 0.22
Si ≤ 0.55 +0.05 ≤ 0.60
Mn ≤ 1.60 +0.06 ≤ 1.66
P ≤ 0.025 +0.005 ≤ 0.030
S ≤ 0.015 +0.005 ≤ 0.020
V ≤ 0.150 +0.02 ≤ 0.170
Nb ≤ 0.070 ±0.005 ≤ 0.075 (Table 1 lists Nb to 0.060%; agree above that)
Ti ≤ 0.035 +0.02 ≤ 0.055
Als ≥ 0.015 −0.003 ≥ 0.012
Cr ≤ 0.30 +0.05 ≤ 0.35
Cu ≤ 0.30 +0.05 ≤ 0.35
Ni ≤ 0.30 +0.05 ≤ 0.35
Mo ≤ 0.20 Not listed in Table 1 Agree in contract (alloy-steel Table 2 would give ≤ 0.21)

How to read Table 2. The band is chosen by the Table 1 upper limit. Si ≤0.55% is above 0.37%, so +0.05% applies; Mn ≤1.60% falls in the 0.80–1.70% band, so +0.06%. For one heat an element may deviate in one direction only.

GB/T 222-2025 replaced GB/T 222-2006 on 1 December 2025. One more rule from it matters to buyers: if no reliable heat analysis exists, the product analysis must meet the heat limits with no deviation at all (clause 5.6).

Z-grade plate is cleaner still. GB/T 5313-2023 limits sulfur by heat analysis:

Z grade Heat sulfur, max (%) Reduction of area, avg / single (%)
Z15 0.010 15 / 10
Z25 0.007 25 / 15
Z35 0.005 35 / 25

CEV and Pcm are always worked out from the heat analysis, not the product analysis. SHH STEEL prints the heat values used and adds a product-analysis column on request. This is building steel, not boiler chemistry such as GB/T 713 Q345R in GB/T 713.

Mechanical Properties

Values below follow Table 3 and Table 5 of GB/T 19879-2023 for Q355GJ, the 2023 name of Q345GJ. Tensile specimens are transverse; Charpy specimens are longitudinal.

Thickness Upper yield ReH (MPa) Tensile Rm (MPa) Yield ratio, max Elongation A, min
6 – 16 mm ≥ 355 490 – 610 0.83 22%
> 16 – 100 mm 355 – 475 490 – 610 0.83 22%
> 100 – 150 mm 335 – 455 470 – 600 0.83 22%
> 150 – 200 mm 325 – 445 470 – 600 0.83 22%

For orders to the 2015 edition, Q345GJ uses lower yield ReL and these bands, with yield ratio ≤ 0.80 and A ≥ 22%:

Thickness (2015) ReL (MPa) Rm (MPa)
6 – 16 mm ≥ 345 490 – 610
> 16 – 50 mm 345 – 455 490 – 610
> 50 – 100 mm 335 – 445 490 – 610
> 100 – 150 mm 325 – 435 470 – 610
> 150 – 200 mm 305 – 415 470 – 610
Test Q345GJB requirement
Charpy V-notch, longitudinal +20°C, KV2 ≥ 47 J, average of 3
Single value One value may fall below the average requirement, not below 70% of it (GB/T 17505)
Sub-size specimens 7.5 mm or 5 mm wide when plate is too thin: 75% or 50% of the required energy
180° bend Per Table 6 to GB/T 232; may be omitted when the mill guarantees it (7.4.3.2)
Through-thickness (≥ 15 mm) Z15, Z25 or Z35 to GB/T 5313, when ordered

Density for theoretical weight is 7.85 g/cm³.

Q345GJB vs Q355B and Q345B: Building Plate or General Structural Plate?

Q345B was the GB/T 1591-2008 name. GB/T 1591-2018 replaced it with GB/T 1591 Q355B. Q345GJB is a different book again: GB/T 19879, written for building frames. Buyers mix the three up every week.

The general structural grade is sold on its minimum yield. The building grade is sold on control: a yield ceiling, a yield-ratio cap, a CEV limit, lower P and S, and 47 J impact. In a seismic frame those rules decide where the steel yields first.

Property Q355B (GB/T 1591-2018) Q345GJB (GB/T 19879-2015) Q355GJB (GB/T 19879-2023)
Yield at 16 mm 355 MPa 345 MPa 355 MPa
Yield at 40–63 mm 335 MPa min 345–455 MPa (to 50 mm) 355–475 MPa
Yield at 80–100 mm 315 MPa min 335–445 MPa 355–475 MPa
Yield upper limit None Yes (110 MPa window) Yes (120 MPa window)
Yield ratio No limit ≤ 0.80 ≤ 0.83
Tensile, to 100 mm 470 – 630 MPa 490 – 610 MPa 490 – 610 MPa
Impact +20°C, 34 J +20°C, 47 J +20°C, 47 J
P / S, max Per GB/T 1591 grade 0.025 / 0.015% 0.025 / 0.015%
Maximum thickness 250 mm (AR tables) 200 mm 200 mm

Q345GJB can replace Q355B in almost every case. Q355B cannot replace Q345GJB: its certificate never reports a yield ratio or a GJ CEV band.

For non-seismic members in heated buildings, GB/T 1591 Q355B is usually enough and costs less. For moment-frame columns and link beams, keep Q345GJB or Q355GJB.

Q345GJB vs Q355GJB: What Changed in GB/T 19879-2023

GB/T 19879-2023 replaced the 2015 edition on 1 April 2024 and renamed Q345GJ to Q355GJ. Chemistry is identical. Strength and ratio rules are not, and that is what decides whether one certificate can serve both names.

Rule Q345GJB (2015) Q355GJB (2023)
Yield measured as Lower yield ReL Upper yield ReH
6 – 16 mm ≥ 345 MPa ≥ 355 MPa
> 16 – 50 mm 345 – 455 MPa 355 – 475 MPa
> 50 – 100 mm 335 – 445 MPa 355 – 475 MPa
> 100 – 150 mm 325 – 435 MPa 335 – 455 MPa
> 150 – 200 mm 305 – 415 MPa 325 – 445 MPa
Tensile, to 100 mm 490 – 610 MPa 490 – 610 MPa
Yield ratio ≤ 0.80 ≤ 0.83
CEV ≤ 50 mm (AR/CR/N) 0.42% 0.43%
Impact +20°C, 47 J +20°C, 47 J
Delivery codes WAR, WCR, N, TMCP AR, CR, NR, N, TMCP

The trap is the overlap. A Q355GJ plate at 470 MPa yield or a 0.82 ratio passes 2023 but fails a 2015 Q345GJ order. A Q345GJ plate at 350 MPa passes 2015 but fails 2023.

When a drawing still says Q345GJB, we ask which edition the reviewer will use. If both, we dual-certify only plate that sits inside both windows: 355–455 MPa yield (to 50 mm) and a ratio of 0.80 or lower.

Q345GJB, Q345GJC, Q345GJD or Q345GJE: Which Quality Grade?

Grade Impact temperature Energy, min C / P / S max (%) Typical use
Q345GJB +20°C 47 J 0.20 / 0.025 / 0.015 Heated interiors, mild climates
Q345GJC 0°C 47 J 0.20 / 0.025 / 0.015 Cold regions, exposed frames
Q345GJD −20°C 47 J 0.18 / 0.020 / 0.010 Severe winters, thick welded nodes
Q345GJE −40°C 47 J 0.18 / 0.020 / 0.010 Arctic and low-temperature sites

Strength, yield ratio and CEV do not change from B to E. Only the impact temperature and the D/E chemistry move. The letter should follow the coldest temperature the steel will see, during erection as well as in service.

Q345GJB is the right letter only when the lowest temperature the steel will see stays well above freezing. For the same letter at another strength level: one level up, Q390GJB; one level down, Q235GJB.

Q345GJBZ15, Q345GJBZ25 and Q345GJBZ35: Through-Thickness Plate

Lamellar tearing starts inside the plate, parallel to the surface, when a large weld pulls on it through the thickness. Box-column diaphragms and T-joints on thick flanges are the classic cases. A Z grade is the guarantee against it.

The designation adds the Z level to the grade, for example Q345GJBZ25. Z tests apply to plate 15 mm and thicker and follow GB/T 5313-2023.

Z grade Heat sulfur, max (%) Reduction of area, avg / single (%)
Z15 0.010 15 / 10
Z25 0.007 25 / 15
Z35 0.005 35 / 25

B and C chemistry allows S up to 0.015%, so even Z15 needs extra desulfurization.

GB/T 19879-2023 clause 7.6 requires every Z plate to be ultrasonic tested one by one to GB/T 2970, acceptance level III. Z35 costs most: lowest sulfur, more rejects, and a Z test on each plate.

Our advice: mark Z25 or Z35 on the cutting list by member, not on the whole order. Stiffeners and webs rarely need it.

Equivalent Material Grades

The nearest foreign building steel is JIS G3136 SN490, which also caps yield and yield ratio. ASTM A992 is the US seismic shape grade with a 0.85 ratio cap; it is a section standard, not plate.

Designation Region Standard Notes
Q345GJB China GB/T 19879-2015 Grade on this page
Q355GJB China GB/T 19879-2023 Current name; see the 2015/2023 table
SN490B Japan JIS G3136 Closest building steel: yield range, ratio ≤ 0.80, Z option
EN 10025-2 S355JR Europe EN 10025-2 Strength and temperature comparison only
EN 10025-2 S355J2 Europe EN 10025-2 40 J / 27 J at −20°C
JIS G3106 SM490B Japan JIS G3106 No yield-ratio rule
ASTM A572 Gr.50 USA ASTM A572 345 MPa; no impact or ratio rule
ASTM A709 Grade 50 USA ASTM A709 Bridge grade; toughness by zone
DIN 17100 St52-3 Germany DIN 17100 (withdrawn) Legacy name

For plate certificates on EN projects, EN 10025-2 or EN 10025-3 plate with EN 10164 Z grades is the usual route. We dual-certify only when both books pass, and say so on the MTC.

Weldability

GB/T 19879 makes the mill calculate CEV from the heat analysis and print it, together with the elements used, on every Q345GJB certificate:

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15

Pcm = C + Si/30 + Mn/20 + Cu/20 + Ni/60 + Cr/20 + Mo/15 + V/10 + 5B

Delivery condition CEV ≤ 50 mm CEV > 50 – 100 mm CEV > 100 – 150 mm CEV > 150 – 200 mm Pcm ≤ 50 mm Pcm > 50 – 100 mm Pcm > 100 – 150 mm Pcm > 150 – 200 mm
AR, CR, NR, N (2023) 0.43 0.45 0.46 0.47 0.26 0.29 0.30 0.30
TMCP (2023) 0.38 0.40 By agreement — 0.24 0.26 — —
WAR, WCR, N (2015, Q345GJ) 0.42 0.44 0.46 0.47 — — — —

At 0.43% CEV (2023, ≤50 mm) Q355GJ welds with ordinary structural procedures. Preheat climbs with thickness and restraint; plate over 50 mm in box columns is where most shops start preheating as routine.

B/C chemistry allows C up to 0.20%. Check actual CEV on the MTC, not the table limit, when setting preheat.

Typical consumables: E50-class low-hydrogen electrodes (E5015/E5016) or ER50-6 wire; AWS E7018 / ER70S-6. Shops work to GB 50661 or AWS D1.1. Write the CEV basis (actual heat, not table maximum) into the WPS.

Heat Treatment and Delivery Condition

Q345GJB/Q355GJB may be delivered AR, CR, NR or N, or TMCP. In the 2015 text the codes were WAR (hot rolled), WCR (controlled rolled), N and TMCP.

Up to about 60 mm most plate ships CR or TMCP. Thick column plate and Z35 plate often ship normalized, which evens out properties through the thickness.

The GB/T 1591 grades with fixed delivery routes are GB/T 1591 Q355NC (normalized) and GB/T 1591 Q355MC (TMCP); compare with EN 10025-3 S355N and EN 10025-4 S355M in Europe.

Test lots follow clause 9.2 of GB/T 19879-2023; retests and judgement follow GB/T 17505.

Dimensions

Q345GJB sizes we supply from mill and stock:

  • Thickness: 6 mm – 200 mm; most orders 10 mm – 120 mm
  • Width: 1500 mm – 3000 mm standard; wider by mill confirmation
  • Length: 3000 mm – 12000 mm; longer by enquiry
  • Edge: mill edge or cut edge
  • Weight: theoretical, on the mean of maximum and minimum thickness, 7.85 g/cm³

Column flanges, diaphragms, stiffeners and gussets are cut to drawing. Rolled sections for the same frame are under steel beam profiles and steel structural profiles.

Tolerances

Dimensional tolerances for Q345GJB come from GB/T 709-2019, as GB/T 19879 directs. The default is Class B, which fixes the minus side at 0.30 mm. Ask for Class C if the design cannot accept any minus.

Nominal thickness (mm) Width ≤ 1500 mm Width > 1500 – 2500 mm
> 8 – 15 −0.30 / +0.80 −0.30 / +1.00
> 15 – 25 −0.30 / +1.00 −0.30 / +1.20
> 25 – 40 −0.30 / +1.10 −0.30 / +1.30
> 40 – 60 −0.30 / +1.30 −0.30 / +1.50
> 60 – 100 −0.30 / +1.50 −0.30 / +1.80
> 100 – 150 −0.30 / +2.10 −0.30 / +2.50

Plate over 150 mm follows the heavier rows of GB/T 709; we state the figures on the offer. Flatness and width follow GB/T 709. EN 10029 or ASTM A6 tolerances are possible if written on the order.

Supplementary Requirements

Q345GJB already fixes strength, yield ratio, CEV and +20°C impact. Anything more goes on the purchase order.

  • Edition: GB/T 19879-2015 (Q345GJ) or -2023 (Q355GJ). Never write only Q345.
  • Product analysis: ask for a second chemistry column checked to GB/T 222.
  • Through-thickness: add Z15, Z25 or Z35, e.g. Q345GJBZ25.
  • Delivery condition: name it (AR, CR, NR, N or TMCP) if the welding procedure depends on it.
  • Ultrasonic testing beyond Z plates: GB/T 2970 class, or EN 10160 / ASTM A578.
  • Impact: extra test positions (e.g. quarter thickness) or transverse tests, if the owner wants them beyond the B letter.
  • Tolerance: Class C for zero minus.
  • Inspection: EN 10204 3.2 with SGS, BV, TÜV or a named inspector.

Q345GJB Price Factors and How to Order

Two Q345GJB quotes can differ by a lot and both be fair. The base price is similar across mills; the extras below are where they part.

Cost driver Effect on price
GJ grade over general Q345 plate Grade extra for cleaner steel, yield control and CEV
Quality letter B No low-temperature extra; B is the base letter
Delivery route N and TMCP carry extras over AR/CR
Thickness Thin and very thick plate carry size extras; 10–60 mm is usually cheapest
Z15 / Z25 / Z35 Desulfurization, plate-by-plate Z test and UT; Z35 costs most
Width and length Over 3000 mm wide or 12 m long needs mill confirmation
Quantity per size Mill rolling minimums per size; small lots come from stock or combined rolling
Inspection and cutting 3.2 witness, profile cutting, blasting and priming are quoted per item

To get a firm quote in one round, send:

  • Grade and edition, e.g. Q345GJBZ25 to GB/T 19879-2015
  • Thickness × width × length and pieces or tonnes
  • Delivery route, UT standard and class
  • Certificate type and inspector
  • Destination port and Incoterm

We quote plate price, extras and freight line by line, so you can compare like with like. Need a different letter? See Q345GJE.

Applications

Sector Typical Q345GJB components
High-rise towers Box and H column plates, transfer girders, outrigger webs
Airports and stadiums Long-span roof trusses, tree columns, node plates
Seismic frames Beam-to-column panel zones, links, brace gussets
Industrial buildings Heavy crane girders, column bases
Bridges in buildings Skybridges, podium transfer trusses

B grade belongs indoors, in heated or temperate conditions, where neither erection nor service sees frost.

It is the wrong plate for pressure equipment (pressure vessel steel plates), for bare exposed steel (weathering steel plates) or for ship hulls (shipbuilding steel plates).

Supply Capability and Global Delivery

SHH STEEL sources Q345GJB from first-line building-steel mills: Wuyang (Wugang), a drafting mill of GB/T 19879, plus Xinyu, Valin Xiangtan, Shougang, Puyang and Hongchang when size requires.

  • Certificates: EN 10204 3.1 standard; 3.2 with third-party witness
  • Tests: tensile, +20°C Charpy, bend, Z test to GB/T 5313, UT to GB/T 2970, product analysis
  • Processing: CNC plasma and flame cutting, bevelling, drilling, shot blast and primer
  • Terms: FOB Shanghai, CFR, CIF; TT, LC or TT + LC
  • Marking: steel-stamped and paint-marked with grade, heat, size and mill

Q345GJB leaves Shanghai for projects designed to Chinese codes abroad, mostly through EPC contractors in Southeast Asia, the Middle East and Africa. We also ship ASTM, ASME, EN, DIN and JIS plate to Europe and the Americas.

Lead time: stock sizes about 5–7 days (B/C letters); mill rolling about 30–45 days; Z35 or 3.2 inspection adds about 1–2 weeks. Sea time from Shanghai is about 7–12 days to Singapore and 28–35 days to Rotterdam.

Why Choose SHH STEEL

SHH STEEL works mill-direct as a steel manufacturer and exporter and global steel mill sourcing partner, China origin. With Q345GJB you get the GJ plate the drawing asks for, traced to the heat.

Before shipment we check four lines on every certificate: yield inside the GJ window, yield ratio within the cap, CEV inside the thickness band for the delivery route, and +20°C impact at 47 J or more. If one fails, the plate does not ship as GJ.

We also tell buyers when they are over-specifying. If the member is outside the lateral system, GB/T 1591 Q355C may be enough, and we will tell you. Browse more structural steel plates and high strength low alloy plates.

FAQ

What is Q345GJB steel?
Q345GJB is building structure steel plate to GB/T 19879-2015 with 345 MPa minimum yield, a 110 MPa yield window, yield ratio ≤0.80, CEV limits and Charpy impact of at least 47 J at +20°C. GB/T 19879-2023 renamed it Q355GJB, with 355–475 MPa yield and a 0.83 ratio cap.
What is the difference between Q345GJB and Q355B?
Q355B is general structural plate to GB/T 1591-2018 with a minimum yield that falls with thickness and no yield cap or ratio limit. Q345GJB is building plate to GB/T 19879 with a capped yield window, a yield ratio of 0.80 (2015) or 0.83 (Q355GJB, 2023), CEV limits and 47 J at +20°C. Q345GJB can replace Q355B; the reverse needs designer approval.
Can Q345GJB be used for outdoor steelwork?
Only where neither erection nor service goes below about 0°C. Grade B proves 47 J at +20°C and nothing colder. For frames exposed to frost, order Q345GJC (0°C), Q345GJD (−20°C) or Q345GJE (−40°C); the strength, yield cap and ratio limit stay the same.
Is Q345GJ the same as Q355GJ?
Not exactly. Q355GJ is the GB/T 19879-2023 name for the former Q345GJ. Chemistry is the same, but Q355GJ has a higher minimum yield (355 vs 345 MPa), a wider yield window (355–475 vs 345–455 MPa to 50 mm) and a looser yield ratio cap (0.83 vs 0.80).
What is the difference between heat analysis and product analysis for Q345GJB?
Heat analysis is taken from the molten steel and must meet GB/T 19879 Table 1. Product analysis is taken from the finished plate and may exceed Table 1 by the permitted deviations of GB/T 222, for example +0.005% for P and S. CEV is always calculated from the heat analysis.
What is the ASTM or EN equivalent of Q345GJB?
The current Chinese name is Q355GJB (GB/T 19879-2023). Abroad, the closest building steel is JIS G3136 SN490B. EN 10025-2 S355JR and ASTM A572 Gr.50 match strength only: they have no yield cap or yield-ratio limit, so they are not direct substitutes.

Conclusion

Q345GJB steel plate to GB/T 19879 is building structure plate with 345 MPa (2015) or 355 MPa (2023, as Q355GJB) minimum yield, a capped yield window, a yield-ratio limit and 47 J impact at +20°C. It shares its chemistry with Q345GJC but proves toughness at its own letter. It is not general structural plate under GB/T 1591.

Every Q345GJB plate from SHH STEEL ships with heat analysis, CEV, yield and yield ratio, and Charpy results on an EN 10204 3.1 or 3.2 certificate. Product analysis to GB/T 222, Z15–Z35, UT to GB/T 2970, Class C tolerance and cut-to-size are options.

We ship from Shanghai to buyers worldwide. Browse the full GB/T 19879 range or other carbon steel plates.

Share your size list, Z level, quality letter and the edition on the drawing, and we reply with the mill, delivery route, lead time, test plan and price in one message. Contact SHH STEEL for a mill-direct Q345GJB building steel plate quotation.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X