New Products /back


S355M EN10025-4 S355M steel plate

2011年4月5日 by admin

EN10025-4,S355M,S355M steel,S355M steel grade,S355M steel plate.

 

Adopt Standard EN10025-4

Gang steel Grade:

EN10025-4

S275M

S275ML

S355M

S355ML

Grade

S420M

S420ML

S460M

S460ML

 

S355M steel plate

S355M Grade is a technical delivery conditions for thermo mechanical rolled weldable fine grain structural steels.
S means the structural steel, M means the delivery condition.
Capital letter L for the quality with specified minimum values of values of impact energy at temperature not lower than -50 degree.

 

Gangsteel is a large agent of HBIS wuyang mill in China and we are specialized in super thick S355M steel plate. We could supply the min order is a piece and promise the competitive price in order to enlarge our oversea market.

S355M Chemical composition of the product analysis for thermo mechanical rolled steel

Element

S355M  Max %

Element

S355M max %

C

0.16

AL

    0.015 min

Si

0.55

TI

0.06

Mn

1.70

CR

0.35

P

0.035

NI

0.55

S

0.030

Mo

0.13

Nb

0.06

Cu

0.60

V

0.12

N

0.017

 

S355M Mechanical properties at ambient temperature for thermo mechanical rolled steel

Grade

Thickness

Yield Strength

Tensile Strength

Elongation

Impact Energy

(mm)

MPa (min)

MPa

% (min)

(KV J) (min)

 

 

 

 

-20 degree

S355M

≤ 16

355

470-630

22

40

16> to ≤40

   345

470-630

22

40

40> to ≤63

335

450-610

22

40

63> to ≤80

325

440-600

22

40

80> to ≤100

325

440-600

22

40

100> to ≤120

320

430-590

22

40

 

If you want to find our stock in S355M, or inquiry S355M from our Gangsteel, please feel free to contact us by email or calling.